Re: [MW:4126] Preparation of WPS

Yes,
 
The WPS can be prepared . However as the material is not included in QW 422 so the WPS will be  specific to material grade used in procedure qualification.
 
amarjit Singh
TEMA INDIA LTD
 
On 1/21/10, GOPU NAIR <gopunair5343@yahoo.com> wrote:
Dear All
 
Recently I have qualified a WPS on 20mm thick plate of EN10025 S355J2G3 using GTAW for root pass and SMAW for subsequent passes in accordance with Lloyds Register Rule for ship building.  The test piece has undergone Tansverse tensile test (2), Side bends (4) Impact test (3 Sets)  at centre of the weld, fusionline and HAZ at -20deg.C, Macro and Hardness (1). PT and RT were carried out the test samples prior to drawing the destructive test samples.  all the tests are passed with the required values. Record of welding for each run is prepared and maintained.
 
consumable used are ER70-S2 and E-7018-1
Plate material properties are: Yield 357 N/MM2, UTS 541 N/MM2, El;  30% IMPACT at -20deg C; 53min, 81 Av.
C;0.18, Si: 0.35 Mn ;1.4, P    ;0.015, S : 0.002 Ce; 0.428
 
PQR as per the Lloyds rules is under preparation.
 
My question is whether I can prepare a WPS and PQR in accordance with ASME Sec. IX using the above records.
 
Regards
 
Gopu/CEPL
 
 
 


The INTERNET now has a personality. YOURS! See your Yahoo! Homepage.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.




--
Amarjit Singh

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...