Skip to main content

Re: FW: [MW:4165] Underclad cracking tests

Dear Nautiyal,
 
Hydrogen disbonding test is conducted as per ASTM G146. After cladding LAS with required WOL(SASC 309L(cb) +347L in your case) the specimenn is prepared as mentioned in G146 & Ultrasonically tested. The test is conducted by Mettalurgical Lab in Mumbai in India and take 10days approx.
 
amarjit Singh

 
On 1/29/10, PREM SHANKARDUTT NAUTIYAL <prem_nautiyal@rediffmail.com> wrote:
Dear Sir

We have to deposit min. 6mm overlay by SASC on LAS - shell & Dish end I.D.
First layer is by 309L(Cb) and subsequent layers by 347L.

For this it has been specified that Weld specimen for Reheat cracking should be prepared.
The procedure is : do cladding by SASC with high heat input,remove the clad till weld fusion layer is exposed and conduct MPI + Metallography.

We have been told that Hydrogen induced cracking should be checked by welding a 50mm width overlay with E9018G on LAS with low heat input, kept at room temperature for 8-10 days... ( No reference standard is mentioned )

I just needed more detailed information / procedure..

Regards

Prem Nautiyal

On Fri, 29 Jan 2010 08:46:28 +0530 wrote

>

>
>

Hi Prem,

Could you be more specific about your query:-

· Underclad Cracking Test— is it related to SAW strip cladding of S.S / Inconel on Reactor Pressure Vessels (RPV) shells. What kind of reheat cracking tests you have to do? Usually reheat cracking is very difficult to simulate.

· Regarding hydrogen cracking, there are standard tests developed and adopted by the industry. If you are familiar with Tekken Y-Grove test, it's a very popular test for hydrogen cracking. What's the test you're asked to perform in this case.

However underclad hydrogen cracking is a bit different issue. Typically it's commonly performed as autoclave testing, and ASTM –G-146, is the standard followed for this underclad hydrogen disbanding test.

Due to copyright issue, I can not post the ASTM standard. However the attached article tells clearly how this test is performed.

Thanks


Pradip Goswami,P.Eng
Senior Engineer/Specialist(Welding-Metallurgy)
Engineering & Training Services Division
ONTARIO POWER GENERATION Inc.
PO Box-2000, RR-55(South)
Nanticoke, Ontario,N0A1L0
Tel:-(519) 587-2201, Ext 3107--in Nanticoke
(416) 231-4111, Ext 5925--in Kipling,Toronto
Fax:(519) 587-6814
Email-pradip.goswami@opg.com.




From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of PREM SHANKARDUTT NAUTIYAL
>Sent: Wednesday, January 27, 2010 1:20 PM
>To: materials-welding@googlegroups.com
>Subject: *****SPAM***** [MW:4160] Underclad cracking tests

Dear All
>
>Can anyone provide some article / explanation / detailed procedure about how to prepare specimens and conduct test for the following Underclad cracking test ---

>1)Weld specimen for reheat cracking.
>2)weld specimen for Hydrogen induced cracking.

>The job is a PV, code of construction is ASME Sec III, NB.
>
>Regards
>
>Prem Nautiyal
>
>PREM S NAUTIYAL
>CELL : 9820313278





--
>To post to this group, send email to materials-welding@googlegroups.com
>To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
>For more options, visit this group's bolg at http://materials-welding.blogspot.com/
>The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.




>
THIS MESSAGE IS ONLY INTENDED FOR THE USE OF THE INTENDED RECIPIENT(S) AND MAY CONTAIN INFORMATION THAT IS PRIVILEGED, PROPRIETARY AND/OR CONFIDENTIAL. If you are not the intended recipient, you are hereby notified that any review, retransmission, dissemination, distribution, copying, conversion to hard copy or other use of this communication is strictly prohibited. If you are not the intended recipient and have received this message in error, please notify me by return e-mail and delete this message from your system. Ontario Power Generation Inc.
>




--
>
To post to this group, send email to materials-welding@googlegroups.com
>
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
>
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
>
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
>


PREM S NAUTIYAL
CELL : 9820313278

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
Amarjit Singh

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...