Skip to main content

FW: [MW:4098] RE: 4089] RE: 4088] Weld Efficiency


 




 

Dear Praphulla,

 

I have attached a schematic for illustration of various joints, for all the forum members. As per Table-UW-12, the joint in question is Type-3, which is single sided butt welds, without backing strips. This kind joint is permitted for type- A (L-Seam), B (Circ-Seam) , Type-C(Mainly Flange Joints).The limitations are specified in Table –UW-12

 

As per UW-12, the minimum efficiency for this type of weld permitted and required for code design is 0.60. One may perform RT over the code requirements but that is optional. From the description it's is Type –B weld on pipe , with the RT criteria specified in UW-11(a) (2).

 

Hence all stand points you may consider this joint as efficiency =.0.60.

 

Thanks

 

Pradip Goswami,P.Eng

Senior Engineer/Specialist(Welding-Metallurgy)

Engineering & Training Services Division

ONTARIO POWER GENERATION Inc.

PO Box-2000, RR-55(South)

Nanticoke, Ontario,N0A1L0

Tel:-(519) 587-2201, Ext 3107--in Nanticoke

          (416) 231-4111  (416) 231-4111 , Ext 5925--in Kipling,Toronto

Fax: (519) 587-6814

Email-pradip.goswami@opg.com.

  


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Bathula Raghuram (Mumbai - PIPING)
Sent:
Tuesday, January 19, 2010 6:40 AM
To: materials-welding@googlegroups.com
Subject: [Norton AntiSpam] [MW:4091] RE: 4089] RE: 4088] Weld Efficiency

I suppose this will be welded by GTAW process to obtain full penetration weld (which will give same quality of weld metal both sides) hence can be considered under type 1.

 

Even I would like to know which type of joint falls under type 3 (in my opinion only those circumferential welds which don't require full penetration), anybody give example?

 


From: Phirke, Praphulla D (GE Infra, Oil & Gas) [mailto:praphulla.phirke@ge.com]
Sent:
Tuesday, January 19, 2010 4:56 PM
To: Bathula Raghuram (Mumbai - PIPING); materials-welding@googlegroups.com
Subject: RE: 4089] RE: 4088] Weld Efficiency

Hi Bathula

Its simple Pipe to pipe joint single butt weld joint ( 4 to 8" Sch 10 pipes) .But considering the thickness & diameter its lying in Type 3.

Can we consider Type 1, but its for double weld butt joints?

 

Thanks

Praphulla

 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Bathula Raghuram (Mumbai - PIPING)
Sent:
Tuesday, January 19, 2010 4:50 PM
To: materials-welding@googlegroups.com
Subject: [MW:4089] RE: 4088] Weld Efficiency

What type of joint it is, if it is to be radiographed, why not consider under type 1 of table UW12

 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Phirke, Praphulla D (GE Infra, Oil & Gas)
Sent:
Tuesday, January 19, 2010 4:30 PM
To: materials-welding@googlegroups.com
Subject: [MW:4088] Weld Efficiency
Importance: High

Hi All

As per ASME SEC VIII Div I, in Table UW-12 , for type No 3 weld joints, 0.7 joint efficiency is specified without any radiographic examination.

But If I performed radiography examination, then what joint efficiencies values I should consider for Full & Spot radiography? As per code & Table UW-12, its NA. 

 

Please guide me.

 

Thanks 

Praphulla D. Phirke 

Lead Engineer

GE Infrastructure

Oil & Gas

ASE-RC PV & HEX

John F. Welch Technology Centre

 

T    + 91-080-4088 5903  + 91-080-4088 5903

F   + 91-080-2841 2111

M   + 91-9886052515  + 91-9886052515

praphulla.phirke@ge.com

 

Odyssey, Phase - 5, Wing A, 2nd Floor,

Plot No 122, EPIP Phase II,

Whitefield Road, Bangalore 560 066

GE India Technology Center Pvt. Ltd.

 

GE imagination at work

 





THIS MESSAGE IS ONLY INTENDED FOR THE USE OF THE INTENDED RECIPIENT(S) AND MAY CONTAIN INFORMATION THAT IS PRIVILEGED, PROPRIETARY AND/OR CONFIDENTIAL. If you are not the intended recipient, you are hereby notified that any review, retransmission, dissemination, distribution, copying, conversion to hard copy or other use of this communication is strictly prohibited. If you are not the intended recipient and have received this message in error, please notify me by return e-mail and delete this message from your system. Ontario Power Generation Inc.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...