Re: [MW:35251] Overlay welding defects

Dear sir,

Thanks for your valued feedback.Details given below.

Stick out                     - 5 to 7.0mm
Gas flow Rate            - 15 to 20 lpm
Ams                            - 175 to 190 Ams
Voltage                       - 23-26V
Nozzle Gas cup size  - 14mm
Travel Speed             - 130 to 160
Oscillation Width       - 8mm

Regards,
R.Gowtham.


On Thu, Sep 12, 2024 at 6:15 PM sridhar cn <sridharcn305@gmail.com> wrote:
The pores in the photos point to the shielding gas issue only. 
It could be due to: 
a contamination in the gas or the filler wire
an insufficient gas flow rate,
a higher flow rate creating turbulence drawing outside air into the welding area,
Gas line leaks or solenoid valve leaks thereby reducing the gas flow,
a higher stick out for the filler wire,
air draft disrupting the flow of shielding gas, 
a faster travel speed, 
a defective gun nozzle,
The weld nozzle held too far away from the well puddle,
a wider nozzle (use 14 or 16 mm nozzle) opening like 20 to 22 mm,
the gun being laid at an angle that sucks in air from the backside.

Please check the above points. 
You have not sent the stick-out used and other parameter details yet.
Sridhar.
------------------------------------------------------------------------------------------






On Wed, 11 Sept 2024 at 14:04, Karthick Flow Controls <kfccovaigm@gmail.com> wrote:
Dear sir,

Photo attached.




Regards,
R.Gowtham.

On Wed, Sep 11, 2024 at 1:48 PM Karthick Flow Controls <kfccovaigm@gmail.com> wrote:
Dear Sir,

The below is another type of defect,Mostly these two type of defects we faced.





Regards,
R.Gowtham.

On Wed, Sep 11, 2024 at 1:42 PM Karthick Flow Controls <kfccovaigm@gmail.com> wrote:

 Sir,

The above photo is one sample.


Regards,
R.Gowtham.




On Tue, Sep 10, 2024 at 4:17 PM sridhar cn <sridharcn305@gmail.com> wrote:
Mr. Gowtahm,
Using an LPG burner or furnace is fine. Argon gas supplier is OK. 
Please send a photo of your defects and setup if possible and weld parameters like ampere, 
voltage, stick-out, travel speed (not rotation time), torch angle if you are using an SPM, gas 
flow rate, oscillation width, and position of the contact tip in the nozzle (is it inside or 
outside—if so, how much, type/make of the welding equipment, nozzle opening, etc. to 
diagnose the issues. 
Sridhar.


On Tue, 10 Sept 2024 at 11:39, Karthick Flow Controls <kfccovaigm@gmail.com> wrote:
Dear sir,

Thank you for your feedback sir.

We use LPG Cylinder for Preheat dia above 1000mm,We use Furnace for Small sizes.
Argon Gas Used Praxair ( Linde).
The below points,We will check in the Process.
If you are using the GMAW process, make sure to keep a lower stick out and the correct amount of shielding 
gas flow rate. A very low/high gas flow rate or welding without a flow meter may also induce porosity. 
Make sure not to open the Argon cylinder fully, as it may increase gas flow velocity and may induce pinholes.

Mainly the defect is noticed in the Bore bottom Radius Area ,Second one Continuous dotted line in the Overlapping.


Regards,
R.Gowtham.



On Mon, Sep 9, 2024 at 5:44 PM sridhar cn <sridharcn305@gmail.com> wrote:
Mr. Gowtham,
These sorts of problems are common in overly welding. 
Please make sure that jobs are preheated properly (not with Oxy-fuel gas; it may create pinholes) 
using LPG, according to your WPS.
Make sure that the Argon gas is procured from a reputed brand and not from a local manufacturer
as it may not be pure even though certified for a 99.99% purity level.
The overlay should not be done in an open area where air circulation is more and should be well-protected 
from fan breeze, etc.
If required, use UHP Argon (99.999% pure), but it will be very costly.
GTAW and plasma arc welding could be more appropriate for the overlay technique.
If you are using the GMAW process, make sure to keep a lower stick out and the correct amount of shielding 
gas flow rate. A very low/high gas flow rate or welding without a flow meter may also induce porosity. 
Make sure not to open the Argon cylinder fully, as it may increase gas flow velocity and may induce pinholes.
Hope the above information will be of help to you.
C Sridhar.
--------------------------------------------------------------------------------------------------------




































properly according to your WPS.


On Mon, 9 Sept 2024 at 10:57, Karthick Flow Controls <kfccovaigm@gmail.com> wrote:
Dear sir,

Welding Valve body & Adapter,(Ball Valve,Triple offset Butterfly,Trunnion mounted Ball Valve & Top Entry Ball Valve.


Regards,
R.Gowtham.

On Fri, Sep 6, 2024 at 11:21 AM Mohd Siraj <mohd52100@gmail.com> wrote:
WCB/LCB fitting elbow or tee components, pl follow,

weld with CS filler wire first then start overlay.

On Thursday, September 5, 2024 at 11:07:20 AM UTC+3 Karthick Flow Controls wrote:


Inconel 625 & 316L -GMAW
Shielding Gas - Argon 
Position -1G


Regards,
R.Gowtham.

On Wed, Sep 4, 2024 at 4:08 PM 'J Prinsen' via Materials & Welding <material...@googlegroups.com> wrote:
First questions: which process, which shielding gas, which welding position, which welding parameters

Regards

Jurgen Prinsen IWE
Weld-Tech BV
Welding Engineering and Consultancy


Van: "Karthick Flow Controls" <kfcco...@gmail.com>
Aan: "Materials & Welding" <material...@googlegroups.com>
Verzonden: Woensdag 4 september 2024 07:26:39
Onderwerp: [MW:35217] Overlay welding defects

Dear Experts,
Welding Overlay, After Machining the Pin holes and blow holes noticed in Overlapping Joint area, After attend the defects, It will open some other places, The defects noticed Uniform inline.   ( Overlay Material ,316L ,Inconel 625 ,St6 & ST21,Base Material WCB/LCB),
How to prevent the defects?




Regards,
R.Gowtham.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/33a4e532-e9d1-45f0-a35f-2172b2263b12n%40googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.


--

Thanks & Regards,
R.GOWTHAM.
KARTHICK FLOW CONTROLS, 
1/575 SNMV College Road, 
Mallumichampatti,
Coimbatore - 641 050.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/287ab92f-439c-461a-9c0d-6a9c21ca53abn%40googlegroups.com.


--

Thanks & Regards,
R.GOWTHAM.
KARTHICK FLOW CONTROLS, 
1/575 SNMV College Road, 
Mallumichampatti,
Coimbatore - 641 050.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADsiqoGENtjXWAmz5FGB0JFFwQN0GAQ%3Dk9385JFQ-J7cn920tg%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAHo%3DYigTK9QZO4qm5sp4r%2BsamNy1LJ8baGBkepB5RB4qJcR%2Bug%40mail.gmail.com.


--

Thanks & Regards,
R.GOWTHAM.
KARTHICK FLOW CONTROLS, 
1/575 SNMV College Road, 
Mallumichampatti,
Coimbatore - 641 050.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADsiqoF07SUcjCNiusS67UtZfecZYtn4VxbPKYsH7RHgpmt0dg%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAHo%3DYiirjOnqFjq-qf1do4L7JkN7mBi9cutaJDVRnJLgW%3DxzNA%40mail.gmail.com.


--

Thanks & Regards,
R.GOWTHAM.
KARTHICK FLOW CONTROLS, 
1/575 SNMV College Road, 
Mallumichampatti,
Coimbatore - 641 050.



--

Thanks & Regards,
R.GOWTHAM.
KARTHICK FLOW CONTROLS, 
1/575 SNMV College Road, 
Mallumichampatti,
Coimbatore - 641 050.



--

Thanks & Regards,
R.GOWTHAM.
KARTHICK FLOW CONTROLS, 
1/575 SNMV College Road, 
Mallumichampatti,
Coimbatore - 641 050.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADsiqoGBDorZxi2_g4L8P3fxzapjsO0JNEpuNhqpfD_3EJ1hUA%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAHo%3DYihiSyxLzxRVDbk7KnbQmgYvjWoy5GLC1EY5Y_go4s7YbQ%40mail.gmail.com.


--

Thanks & Regards,
R.GOWTHAM.
KARTHICK FLOW CONTROLS, 
1/575 SNMV College Road, 
Mallumichampatti,
Coimbatore - 641 050.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADsiqoHnO_4s%3Da_QczvUJVy3pja694U8Cj0cuK7HcWXcd-RxNg%40mail.gmail.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...