Skip to main content

Re: [MW:35226] Re: Filler wire for 321H

ER 316H lacks the niobium stabilization that 321H requires for high-temperature applications 
and potentially leading to sensitization/reduced corrosion resistance in the heat-affected zone 

ER347 is the preferred filler material.  

On Friday, September 6, 2024 at 7:00:54 AM UTC+3 Mohmmed Dudhiyawala wrote:
Use ER316H.
We are successfully welding S321H, as per Russian GOST codes requirement.

On Wednesday, September 4, 2024 at 4:08:07 PM UTC+5:30 J Prinsen wrote:
Best use ER347H, Nb stabilized 18 10 Cr Ni steel

Regards

Jurgen Prinsen IWE


Van: "Kannayeram Gnanapandithan" <kgpan...@gmail.com>
Aan: "materials-welding" <material...@googlegroups.com>
Verzonden: Vrijdag 30 augustus 2024 10:21:33
Onderwerp: Re: [MW:35204] Re: Filler wire for 321H

ER 5356, is it not aluminium filler??

THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


On Fri, Aug 30, 2024 at 1:36 PM trivikram kommala <trivikra...@gmail.com> wrote:
TIG 404 (ER 5356) - AWS / SFA 5.10



On Friday, August 23, 2024 at 8:07:57 AM UTC+5:30 Vignesh Manoharan wrote:
Hi experts, 

What filler wire is required to weld 321H in GTAW process. ? 

Pls suggest


Regards
Vignesh M

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/a8e117c1-29b0-41aa-a8cf-c5ae26ab6c0an%40googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/56129659-2c4a-43bb-9929-6f919f5f195cn%40googlegroups.com.

Comments

Popular posts from this blog

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...