Skip to main content

Re: [MW:35231] Re: Filler wire for 321H

ER347 is not meeting min C % requirement of 0.4%.
In that case, ER347 cannot be used. then which filler to be used?

On Friday, September 6, 2024 at 11:24:49 AM UTC+5:30 Mohd Siraj wrote:
ER 316H lacks the niobium stabilization that 321H requires for high-temperature applications 
and potentially leading to sensitization/reduced corrosion resistance in the heat-affected zone 

ER347 is the preferred filler material.  

On Friday, September 6, 2024 at 7:00:54 AM UTC+3 Mohmmed Dudhiyawala wrote:
Use ER316H.
We are successfully welding S321H, as per Russian GOST codes requirement.

On Wednesday, September 4, 2024 at 4:08:07 PM UTC+5:30 J Prinsen wrote:
Best use ER347H, Nb stabilized 18 10 Cr Ni steel

Regards

Jurgen Prinsen IWE


Van: "Kannayeram Gnanapandithan" <kgpan...@gmail.com>
Aan: "materials-welding" <material...@googlegroups.com>
Verzonden: Vrijdag 30 augustus 2024 10:21:33
Onderwerp: Re: [MW:35204] Re: Filler wire for 321H

ER 5356, is it not aluminium filler??

THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


On Fri, Aug 30, 2024 at 1:36 PM trivikram kommala <trivikra...@gmail.com> wrote:
TIG 404 (ER 5356) - AWS / SFA 5.10



On Friday, August 23, 2024 at 8:07:57 AM UTC+5:30 Vignesh Manoharan wrote:
Hi experts, 

What filler wire is required to weld 321H in GTAW process. ? 

Pls suggest


Regards
Vignesh M

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/a8e117c1-29b0-41aa-a8cf-c5ae26ab6c0an%40googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/01cf6c3a-931b-4635-86d6-a5189bc7d408n%40googlegroups.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

[MW:30043] Weep hole

If weep hole is not provided in dummy pipe before welding What will happen??? -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/da251ee6-fa7f-4851-b876-cdb3834ae341%40googlegroups.com .