Skip to main content

Re: [MW:32297] Re: Back Weld at Pressure vessel - U stamp

Dear 

 As per ASMe sec IX QW 402  - Joint design - GTAW - Backing - With/Without 

GTAW - QW 402.5- Addition of  backing is Non essential variable.)

if Both (Backing - With/Without  )  must be addressed in your WPS then there is no issue to weld 

Regards
Pravean

On Mon, 19 Apr, 2021, 6:05 pm Ramesh, <rameshkannandevaraj@gmail.com> wrote:

Don't not confuse with production weld and repair welds

 

Though its single sided weld as per WPS for your production ,  when repair comes at root what you do ? ( presuming accessible at root side )

 

For repair, your weld metal is backing material, so any welder qualified with backing or without backing can repair in your case. 


Thanks and Regards

Rameshkannan D

"What you have learned is a mere handful; What you haven't learned is the size of the world – Avvaiyar"




On Mon, Apr 19, 2021 at 5:31 PM Vishwas Keskar <vvkeskar123@gmail.com> wrote:
Dear Samkar

May I know what is your concern now ?

On Mon, Apr 19, 2021 at 3:51 PM sankar bombay <sankar.bombay@gmail.com> wrote:
For GTAW Welder QW-402.4 Deleting of backing is essential Variable 
Addition of backing they have not mention 

On Mon, Apr 19, 2021 at 2:19 PM Ramesh <rameshkannandevaraj@gmail.com> wrote:

Seems weld repair carried out at the root side. Whether your repair carried out as per approved repair procedure ? 

 

With Backing or without backing is essential for welders, not for procedures !

unless there are any specific requirements from the client / inaccessible area for root welding.


Thanks and Regards

Rameshkannan D

"What you have learned is a mere handful; What you haven't learned is the size of the world – Avvaiyar"




On Mon, Apr 19, 2021 at 1:09 PM Vishwas Keskar Welding Manager WELDING <vvkeskar123@gmail.com> wrote:
Is  that WPS  addressing - 
 QW 402  - Joint design - GTAW - Backing - With/Without 
(Ref - QW256- GTAW - QW 402.5- Addition of  backing is Non essential variable.)

if Both (Backing - With/Without  )  is addressed( which  like  normally is  addressed), then there is no issue at  all .

Eg-

QW 402-

Backing: With/Without                                                                         

Root spacing: As per piping fabrication drawing                                                                                                          

Backing Material (Type): Yes (Metal)

1. Metal -        2. Non-fusing Metal      

3.   Nonmetallic NA   4. Others 

The matter is to  be resolved  amicably . Meet QAC  In charge along with Welding Engineer, Manufacturing Responsible. Explain him the details . 
It shall be acceptable.


Regards

On Monday, April 19, 2021 at 7:20:46 AM UTC+4 sankar krishnan wrote:
Dear Gentlemen,

   Good Evening, In our project Vessel joint thickness 10mm ,Process(GTAW+SAW),Single V joint 
They completed Welding ,Few days later during Inspection we observed , They have done Internal Welding of the shell, As per WPS its not shown 

Guys let me Know  its can Accepted or Rejected 

If Rejected , Please send Reference code standards

As per QW 402.5 Joints (Backing its non Essential ),Its mention Backing strip or also back welding 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/960d2caa-6684-4216-b79d-6eb48095898cn%40googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAMaSVcGxuHhMRmyXeJobuwT02Mx8KudViGRskgQuiJNRr6ED%3Dw%40mail.gmail.com.


--
shankar

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAAyDEeYx%2Bjddw7_cQ_J1A7u3Op1N-pk9t%2BcAh7LDxXym8AAA0g%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADder3McUQS%2B%3DqRQppxd1B0SUSi9_P3ycAaUPyMU%2B8E93FpRAA%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAMaSVcH%3DqrTAWpycfZ7nUjMYNX7%2B0MwFcBzzNNUXUXVx4KEkvQ%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CANO0gODPHXtP0YfHo0nEqarjR36OEq5aVFeU_70Wp4RxABoXng%40mail.gmail.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Re: [MW:14950] RE: 14919] Stress relieving Rejected for 5 min less soaking time.

Dear All, I have been a CONSULTANT FOR such problem & my personal opinion is expressed as follow. I fully agree with views expressed so far. But bag to differ that " Code is a law, with engineering judgments. Hence the inspector has the rights to declare that the original HT was inadequate." Inspectors & total industry must resist the "REJECTION" . We as intellectual & having seniority must become practical. How the code will revise???. ANS.: One is experiments (Pure research) & second is such chances that gives opportunity to experiment !!! _______________________________________________________________________________________________ My understanding is that it is P1 material. In that case every pass normalizes the immediate bottom pass. Hence code requirement for P1 FOR MANDATORY SR is 32 mm & above thickness. SOLUTION:  In any case 0. After SR=PWHT no PTC testing is required as per code--Unless for low temp. vessels. That means code ...