Skip to main content

Re: [MW:32267] welding api 5l x52 with x60

Its mean im in safe area to weld x52 with a694 f60 with thé same WPS 

Électrode 6010 with 7018 or er70-s6 with 7018

Le ven. 16 avr. 2021 à 04:18, 'james gerald' via Materials & Welding <materials-welding@googlegroups.com> a écrit :
It is a normal practice in Pipeline to use low tensile electrode for the Root and hence you can use the WPS for welding X52 to A694 F60 as the requirement is the minimum Tensile strength as below. Check the PQR that 95% of UTS 67ksi (X52) is achieved.

For Piping, no issue.


Inline image

Thanks & Regards

J.Gerald Jayakumar



On Thursday, 15 April, 2021, 03:27:13 pm IST, Adnan Ziad <adnanziad49@gmail.com> wrote:


for piprlinre  6010 for root and  7018 fil an cap 
for piping  gtaw er70-s6 + smaw  7018 fil and cap 

Le jeu. 15 avr. 2021 à 10:37, Ramesh <rameshkannandevaraj@gmail.com> a écrit :

May I know what was the consumable used in your X52 WPS ?

Thanks and Regards

Rameshkannan D

"What you have learned is a mere handful; What you haven't learned is the size of the world – Avvaiyar"




On Thu, Apr 15, 2021 at 2:49 PM Adnan Ziad <adnanziad49@gmail.com> wrote:
in my case i have also a wps for piping api 5lx52 to a105 -  can i use it to weld it with a694 f 60 

Le jeu. 15 avr. 2021 à 10:03, Ramesh <rameshkannandevaraj@gmail.com> a écrit :
Sample 
image.png

Thanks and Regards

Rameshkannan D

"What you have learned is a mere handful; What you haven't learned is the size of the world – Avvaiyar"




On Thu, Apr 15, 2021 at 2:20 PM Ramesh <rameshkannandevaraj@gmail.com> wrote:

As per API 1104 , 2013 edn, Clause 5.4.2.2 , you can use the same WPS without requalification. I presume your flange and fittings are having same SMYS ( Specified Minimum Yield Strength)  and similar CEq

 

Requalification is required only when the base metal welding involves less than X42 or greater than X65. In your case this is not applicable.

 

Make sure, Your WPS have mentioned : Qualified Base material X42 Through  X60.

 

            Keeping future qualification purpose, it's better to qualify PQR with X65 material which many customers accept for all lower grades' base metal qualification.

Thanks and Regards

Rameshkannan D

"What you have learned is a mere handful; What you haven't learned is the size of the world – Avvaiyar"




On Thu, Apr 15, 2021 at 1:08 PM QA/QC <adnanziad49@gmail.com> wrote:
Dear master 
i have a approved wps for welding api 5l x52  pipeline and i want to weld a anchor flange x60 is the wps cover it or we should requlaify it again 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/c82adcc6-aec4-4acc-9815-966de7fd1a23n%40googlegroups.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAMaSVcH5UFPQ0a3D0hOGCttar2sHnd5Mu%2Bf8TbA3wX%3DytQ89xw%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CACbfGKf721ygyH03f_PBSpsbeaghjR0grKtccgZgjJTeWz5DBw%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAMaSVcGj5fN8OR_9BU0V9cCpiE6hHbPu6gF7keppe7GkrTa0rg%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CACbfGKcV--J2-OV%2B7oXAVY%3Drhzq%2BChcVbG9j%3DkiJxZ825GBjFw%40mail.gmail.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/79455236.1203584.1618495494208%40mail.yahoo.com.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CACbfGKfH-TQd3uPWrfnehVMgstOoLXcNpnP4XqfTi4ozJupLUg%40mail.gmail.com.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Re: [MW:14950] RE: 14919] Stress relieving Rejected for 5 min less soaking time.

Dear All, I have been a CONSULTANT FOR such problem & my personal opinion is expressed as follow. I fully agree with views expressed so far. But bag to differ that " Code is a law, with engineering judgments. Hence the inspector has the rights to declare that the original HT was inadequate." Inspectors & total industry must resist the "REJECTION" . We as intellectual & having seniority must become practical. How the code will revise???. ANS.: One is experiments (Pure research) & second is such chances that gives opportunity to experiment !!! _______________________________________________________________________________________________ My understanding is that it is P1 material. In that case every pass normalizes the immediate bottom pass. Hence code requirement for P1 FOR MANDATORY SR is 32 mm & above thickness. SOLUTION:  In any case 0. After SR=PWHT no PTC testing is required as per code--Unless for low temp. vessels. That means code ...