Re: [MW:27637] Preheat temp lower limit from min temp teg

Hi,
Assumed your construction code is ASME, according to ASME Sec.IX , QW 406.4, It allows preheat temperature can decrease upto 55 degree C than qualified WPS.  Code just gives recommendation for pre heat temperature of minimum 205 degree C but we should follow as per our engineering practice.i.e set up to 240 to avoid temperature reduce while opening heating pad.
In your case , Please check your thermocouple/monitoring thermo couple positions. It might be attached away from the weld location. And also you said during welding. if so, did you verify the temperature before start weld? Once you open the heating pad for welding, you should verify once again with infrared thermometer at weld location before start weld. If you verified and no way to reduce below the temperature you measured during weld.
If you found the temperature measured is less than 205 degree c you dont start weld.
please set preheat temp. to 230 to 240 atleast so that when you open the heating pad it might not be reduced below 205.
Check monitoring thermo couple location which should be as much closer to weld location and also verify again with infrared thermometer before start weld.

Thanks& Regards,

 

(Karthik)

Karthikeyan.S

QA/QC Manager
Agon Pacific Co.,Ltd.
M: +66-655-174-397, +66-892-512-282

E-mail : karthik6684@yahoo.com



On Thursday, April 5, 2018, 1:28:04 PM GMT+7, Kannayeram Gnanapandithan <kgpandithan@gmail.com> wrote:


what is welding process and code of contrustion

THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  AWS-CWI, CSWIP 3.1,
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349

On Wed, Apr 4, 2018 at 2:11 PM, 'smkabeer ahamed' via Materials & Welding <materials-welding@googlegroups.com> wrote:
Dear sir
Item description evaporator outlet header
Material Sa335 P91
Preheat temp 205 deg c min
Process. Induction heating
During welding preheat temp comes to 197 deg c. Please clarify either it is accepted or not.
If it is Accepted please provide relevent standards.  

Thanks and regards
S.M.Kabeer Ahamed
Quest Pvt Ltd Bangalore
9168605601

--
https://materials-welding. blogspot.com/
https://www.linkedin.com/ groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@ googlegroups.com.
Visit this group at https://groups.google.com/ group/materials-welding.
For more options, visit https://groups.google.com/d/ optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...