Skip to main content

Re: [BULK] [MW:27696] Stainless steel (SA 312 TP 316L) welding

Hi

I did not get any chance to do research on the effect of ferrite content on SS to answer your question exactly,  however I found one welding journal related to this discussion, attached herewith for reference.

Specific case study : The elevated-temperature mechanical properties of weld metal with a wide delta ferrite range are determined following their deposition using E308-16 covered electrodes.

 

There may be many studies available like this

 

There is brief explanation given in TWI page as below link,

https://www.twi-global.com/technical-knowledge/job-knowledge/welding-of-austenitic-stainless-steel-103/






On Wed, Apr 11, 2018 at 5:26 PM, Kannayeram Gnanapandithan <kgpandithan@gmail.com> wrote:
if ferrite is more than 10, what will happen

THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  AWS-CWI, CSWIP 3.1,
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349

On Wed, Apr 11, 2018 at 4:24 PM, George Dilintas <dilintas@gmail.com> wrote:
all this when MDMT is colder that -196degC and if the base metal is 316L and if the process is GTAW or GMAW

2018-04-11 8:34 GMT+03:00 Ramesh <rameshkannandevaraj@gmail.com>:

Hi

ASME Sec VIII Div 1 -2017 edition requirement for FN

UHA – 51 & Fig UHA 51.1











On Wed, Apr 11, 2018 at 9:12 AM, Kannayeram Gnanapandithan <kgpandithan@gmail.com> wrote:
Could you elaborate the mechanism of Hot cracks if ferrite is less than 3

THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  AWS-CWI, CSWIP 3.1,
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349

On Tue, Apr 10, 2018 at 10:10 PM, PREM SHANKARDUTT NAUTIYAL <prem_nautiyal@rediffmail.com> wrote:
Ferrite number less than 3 can result in hot cracks in ASS.

Regards

Prem Nautiyal


PREM S NAUTIYAL
CELL : 9769316004





From: Kannayeram Gnanapandithan <kgpandithan@gmail.com>
Sent: Tue, 10 Apr 2018 18:11:30 GMT+0530
To: materials-welding <materials-welding@googlegroups.com>
Subject: Re: [BULK] [MW:27668] Stainless steel (SA 312 TP 316L) welding


what is the reason for Hot cracking

THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  AWS-CWI, CSWIP 3.1,
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349

On Tue, Apr 10, 2018 at 4:51 PM, Lu, Feng <luf@zachrygroup.com> wrote:

3 ~ 8% ferrite are required in the weld to prevent hot cracking

 

 

Feng Lu, Ph.D., NDE Level III
Metallurgy and Welding Engineer

Zachry Industrial, Inc.
3600 West Sam Houston Pkwy South

Suite 200

Houston, TX 77042

luf@zachrygroup.com
Office: 713.979.2648
Cell: 512 797 5777
www.ZachryGroup.com

This e-mail may contain confidential and privileged material for the sole use of the intended recipient. Any review, use, distribution or disclosure by others is strictly prohibited. If you are not the intended recipient (or authorized to receive for the recipient), please contact the sender by reply e-mail and delete all copies of this message.

 

 

 

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Kannayeram Gnanapandithan
Sent: Tuesday, April 10, 2018 5:56 AM
To: materials-welding <materials-welding@googlegroups.com>
Subject: [BULK]Re: [MW:27666] Stainless steel (SA 312 TP 316L) welding

 

what is the necessity for ferrite testing on 316L


THANKS & BEST REGARDS,

KG.PANDITHAN, BE, IWE,  AWS-CWI, CSWIP 3.1,

CONSULTANT-WELDING & QUALITY

Mobile no: +919940739349

 

On Tue, Apr 10, 2018 at 4:16 PM, Perumal Govindan <perumalgovindan@gmail.com> wrote:

Hi Prasad,

 

Ferrite testing is required when it is mentioned in the Client / Project Welding / Construction Specification.

 

 


With Kind Regards

 

P Govindan 

 

On Tue, Apr 10, 2018 at 11:24 AM, 'Shashank Vagal' via Materials & Welding <materials-welding@googlegroups.com> wrote:

NO

 

On Sunday, 8 April 2018 6:41 PM, Prasad Rode <purode333@gmail.com> wrote:

 

Dear sir,

I am going to do PQR for SA 312 TP 316L pipe to pipe of 6" and 7.11mm thickness.

I want to know that, i have to go for ferrite testing or not ?

If not, when it is essential to ferrite testing?

Regards
Prasad

--
https://materials-welding.blogspot.com/
https://secure-web.cisco.com/1YQnsmRr-GH1GARoxWXMeA5C-zFwTzLoctJUEMDdbzGqdXz0x9TjaAPfvUNCLPyWmBF72X02uczwD2w2oQr4w1WU83Qi9TlzHiZ7Q_m9togWnC_PifpMYG8Noh8ecDgt7Rz98rlzdDCP25FnmnS_fTsbYKEW23twpN4Bzour50n0apwtEnAxZYN9sAWmkWYerjHTOdoPgbEeCq6R1TaDdAKBlmlFHT4VODFg8bxr_Ky0_qRNkuh067eU3nfDwrJG-XJiwtMxynCYDVIZxQz1Fv74pM0X3HjGhj247CNngXDfoNc61SRf3RPhE2b34P5EiGja9P9JH-OsWp5vdlOZ_ev82Kyia9HdDn4kwpU9bD_Y/https%3A//www.linkedin.com%2Fgroups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://secure-web.cisco.com/1-hvkRaP05ZCIdzs4SHsFJNT9bNun5it9Jd9i_VDkw1AUQnt1B_8PvkK-5KPssj1ExOaVPMda4kh79O3-nwhzRckMK5PNlvmAX3tP3s8UcQbpjY4u6F98DxOZ_fH7AtzprQyB5Qhj6i06A2Vtf5DvTMzg0taC8VPuylTiEN6kray-J6mSH7rD5orTEuXBUqWHY0XJTUW8BT0jVxHDa8Mpq1J4R8qbvoEgMl3fZ2yaI2GQWyc57xv9U6uF_6RuNqso_Kl_aOOPXwGTepm00WRQkCkB5IN5Bbp3nDX7n3z5YuRFaa6YDUiw3XQ4qTR9dNndOcf4Tb3V5CqSc8r4GTxyOJ_rqisrNgGsTqnWuuQ8S-A/https%3A%2F%2Fgroups.google.com%2Fgroup/materials-welding.
For more options, visit https://secure-web.cisco.com/11LbN4v-1Vdxbtx9wzmvNLlrp8uw6D66SWirlI5SOn-YhcHDPOM5GhE6va5qKkPm_WjdJVCXM_Ev0AsJwnBggZ71lDFT-ump4X6eoB8B9kDI9imYMY1Egx6DHIGG4asTwbZiikNoMyLvIZn2hRyxaMgkPyo-CYZYNykefeET8HwTcUVqQBEPjS-MTu7OmiuqtRe_zpIH1qMlNrjblAuJjS5Uz1SGGxHGmAE3j0SIPzjn5ZXKATiqNlyDVZxWCkTaz4Cv6gLjf9aK7Sd1OpQJkIAcpioyy8RD5qUkbwU9Ixs21FggLi3SNukHhJ3H-XBnX9R3JDCs3NfgZ3Olgx0BzW2UewBza6kNw3toz3lk6w6E/https%3A%2F%2Fgroups.google.com%2Fd%2Foptout.

 

--
https://materials-welding.blogspot.com/
https://secure-web.cisco.com/1YQnsmRr-GH1GARoxWXMeA5C-zFwTzLoctJUEMDdbzGqdXz0x9TjaAPfvUNCLPyWmBF72X02uczwD2w2oQr4w1WU83Qi9TlzHiZ7Q_m9togWnC_PifpMYG8Noh8ecDgt7Rz98rlzdDCP25FnmnS_fTsbYKEW23twpN4Bzour50n0apwtEnAxZYN9sAWmkWYerjHTOdoPgbEeCq6R1TaDdAKBlmlFHT4VODFg8bxr_Ky0_qRNkuh067eU3nfDwrJG-XJiwtMxynCYDVIZxQz1Fv74pM0X3HjGhj247CNngXDfoNc61SRf3RPhE2b34P5EiGja9P9JH-OsWp5vdlOZ_ev82Kyia9HdDn4kwpU9bD_Y/https%3A//www.linkedin.com%2Fgroups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://secure-web.cisco.com/1-hvkRaP05ZCIdzs4SHsFJNT9bNun5it9Jd9i_VDkw1AUQnt1B_8PvkK-5KPssj1ExOaVPMda4kh79O3-nwhzRckMK5PNlvmAX3tP3s8UcQbpjY4u6F98DxOZ_fH7AtzprQyB5Qhj6i06A2Vtf5DvTMzg0taC8VPuylTiEN6kray-J6mSH7rD5orTEuXBUqWHY0XJTUW8BT0jVxHDa8Mpq1J4R8qbvoEgMl3fZ2yaI2GQWyc57xv9U6uF_6RuNqso_Kl_aOOPXwGTepm00WRQkCkB5IN5Bbp3nDX7n3z5YuRFaa6YDUiw3XQ4qTR9dNndOcf4Tb3V5CqSc8r4GTxyOJ_rqisrNgGsTqnWuuQ8S-A/https%3A%2F%2Fgroups.google.com%2Fgroup/materials-welding.
For more options, visit https://secure-web.cisco.com/11LbN4v-1Vdxbtx9wzmvNLlrp8uw6D66SWirlI5SOn-YhcHDPOM5GhE6va5qKkPm_WjdJVCXM_Ev0AsJwnBggZ71lDFT-ump4X6eoB8B9kDI9imYMY1Egx6DHIGG4asTwbZiikNoMyLvIZn2hRyxaMgkPyo-CYZYNykefeET8HwTcUVqQBEPjS-MTu7OmiuqtRe_zpIH1qMlNrjblAuJjS5Uz1SGGxHGmAE3j0SIPzjn5ZXKATiqNlyDVZxWCkTaz4Cv6gLjf9aK7Sd1OpQJkIAcpioyy8RD5qUkbwU9Ixs21FggLi3SNukHhJ3H-XBnX9R3JDCs3NfgZ3Olgx0BzW2UewBza6kNw3toz3lk6w6E/https%3A%2F%2Fgroups.google.com%2Fd%2Foptout.

 

--
https://materials-welding.blogspot.com/
https://secure-web.cisco.com/15CdaQ7SqBttaMDjEgp4vyA1IIjLruZ4x02m8Ah9pYq6pSUFOK4-lHzhH7m7k9MIiS0unxn4qfOA70v59vOPWRGhNUrugmrLXvQ-X0WNEztRVJR8_iUnWuJL7ZngVRii6W0MHgWbayD58uOybu_o_WS7TXJfyWs-_7Fy3RGrk262seUpeYMyBOkVy6JjNeidtV2NikbqfRJ69VudWHlR7Pj1brCz_pmBZyqwiAvBxYfKg2Uu8IxnyW6iurEV6LnqgTLG1l95kaOCk5T8n2-t1_mZz0HXQowSp2KjuOD4Zb7ZnlfDrumTmHmUIr_DltelYqkudojkTlcFiSo_OS8RBn7ObjA0peImqj_vGZwZA27Y/https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://secure-web.cisco.com/1eRh-wf9X8OZeiSzdXfjjdBsreEz2vw6nypbfDtNb9gF9ga2ioNVBw6jsStnX7fBTJt1ESgLZHyRIrp3TXqnx28FIbMh1w8a3F8es4N0JYiKyPOeTKWWkEa9IIqUXxQ9P-Fjen_zx8xXb2UfxCrDNSatnz7YR3tcclkVDWvUGZWNSCxsHhWey9xdfpJ4q6yxf0Nphl2FTNTbt1uzeSbcMh-d1-maJnFMgDZv-W_0HKTlLLzJOpdn7ZZ0ojXZxwg2PSa2zxDZPuPyT49Qzb49J-Vn5b1A5yVIfU6jLSqX01kz5_VERtpsouoOvlyw_ExjdM_Rz3iU2CvSdWr3y5LILETR4FgI0PysBwPO2uVgBq70/https%3A%2F%2Fgroups.google.com%2Fgroup/materials-welding.
For more options, visit https://secure-web.cisco.com/1Gqw5l2Ew0NnLF9ocT7FiPSzoc7Xh5IXXL0ZUUCS2kBzZm-hHDlnrap_v-m_bjpNstyVad2i7EysoEtlOT4Te7ttRG-bQ3cta-FkTGYTXN1OiukqlCyELfHfF-mW95cAi6BWn-5VkwmqdM0MqNz5GayYxa_NlqaaeBiPR599qfT5pB4k82oN1UntSTlKDSO21R7GS84NHR7QhdtV8Jk8SnQeqMqgFiGqQ0xp6ZLe2oxwCz-6n-dTkyCYepQifCb4HSm2SkrJ5jla3kcWsKsa-GWg2J_u_WEMlfVJBriXkMRO9IQQ_2t-pZATcoezLzmb-EKYYb9PEqDsTxFrV5cu-lMxRMUoWqyFeOy10TFMtT90/https%3A%2F%2Fgroups.google.com%2Fd%2Foptout.

 

--
https://secure-web.cisco.com/1Yekz4_Rk1j5eIKzWu3w3uOI4lY_995nOXaYoO2uO0NGqMQXH-ZV9VapwaVCb3IxXLLVZM8kjdu9fM7j1srk-jOXoitpI_KNfy6y596DmYrln7EAsMlF7l9hPmw01eSNbToT4y3p6Ek5qnqPiaII6IAqGJkGpUWHzaHjuP-_HJSX4av0Zg1TxLLPqX1jOpfkdDwcIKu_Ch0W90jC3sje2nKE3fvQdvq-EYXWuoP2PhBkY0GXwY1i2E3lGsFgt1uDo9QhRi4zd7373nAXJj-tQQipR7ApVH3skfaHyElP254ZeHlSze7RhOtIpzCm5v8VlQA1BgwYbg4CwFlK0wOolWVMJxCeqE-36laFK69SEhm4/https://materials-welding.blogspot.com/
https://secure-web.cisco.com/1T4WuM8lkw7TepJTiGMw6aWBwIYmQBseyjuGtIJoulgjhLZ7EVw-eED0B1_ytTaqgwjwuKfJDC_-XzBITrF66Tr4OYoTqxRHrf5DQUoEx9xJI6uGsnT6T8rqf0HxLaPaKsrwqTgORJ2twvVMj_3SiNnhcIVIjbcKSjdNG1FQeNdUJGX4QZfXdCfYnvWOC5GWgApzenhyd2_29Hux1DpznKaRGakrq7I4wwOMAWVHQWE8OCzrYh7nIOtoZyGlAtn7VO4zhFjdXFddWZv8zbXOxkuYVLcN_iktDQ4QjpF2OH1olC3Yq6cQppUBAbQyMxLeGmFekICOzEPKI77xUxO43Tj1RtqibnEb207n4J3s-0nU/https:%2F/www.linkedin.com%2Fgroups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://secure-web.cisco.com/1Ngm51h-0qXokcX3NLuwji6oaxruW94TI5tEOmO1aty65EiLOKKAcQAr68FvwVf78F6_OtvN32tWU5Lo4oA7s1YkEXv0OHLp81p0sCofVtvL_oIeFWNNKGcv9iMdNcwMXXDzGifLIWiQ48hFHkxVInMwZlGnja2s_d_WvL4H0v6n1hcxmdWA3GGn6jMV6d-GX_POXR9hO9uph_XZEpTi7PoWXy1sD6lkIPzr-5dP_L915H9wV0bQQbrS25sQGTV_SiLNRP6rUQrKepRKanOk-bjnvEJU4he9cvr5z5caUHBx0dzFDnJCTVD8sFrYcqLvuy20Uqus58-v-T5mqQfVcEFY9DZFq4rxHOd50h0hvQLM/https%3A%2F%2Fgroups.google.com%2Fgroup%2Fmaterials-welding.
For more options, visit https://secure-web.cisco.com/1-QRVl4sxcfjWZp6YgOWKAKJzKAlR_7F_l7FBH2DlcrNxj28971TvyG3D9TUY7yjqDSQpFDD1cnUDClMxcS5LTpP2yZTAwaIS0TZaWVPLssYGuKtKb1E0XqENY9Rsfh6_ETm2-nUYG3JD_dMZ2IsaFkhc8gkZ8mttKHmSf7i-6Kp6uRv3mlB43KECYM1LxTVCM82pSlZsp8WEmqWAqKDOL2xJ84gtaQQCIZM7zYrZZN1QEiGHUw5VvY3eT0B7MpjQ_mhtwqJkV4AUGApHdPioxXJ8XxQweNrThd9aGwtrOYaf1lV6zwy9Ub2_nSCbcsN81Tem-OjoMabJVULfpk9qctXstwFam_Z-NakErpuQk7w/https%3A%2F%2Fgroups.google.com%2Fd%2Foptout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https:roups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.



--
Dr. Georgios Dilintas,
Dipl. Ing. In Aeronautic and Space Engineering
Ph.D in Mechanics of Solids - Computational Mechanics
A.I.S, A.N.I, IRCA Lead Auditor
Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...