Skip to main content

Re: [MW:26952] RE: Heater coil welding getting Crack - Reg

Normally cracking in Austenitic stainless steels may be Solidification cracking. Solidification cracking occurs because of below reasons.

1. Presence of Impurities like Sulphur, Lead, Arsenic etc..
2. Weld Bead i.e Width to Depth Ratio
3. Time duration between Liquidus and Solidus curve during cooling.

But I do not think the cracking being discussed is Solidification cracking as this type of cracks occurs in crater with Branches.

I feel this cracking at start and End  is due to Welder or Technique. Sudden removal of Filler creates shrinkage stresses which results in cracking and I suppose it is due to shrinkage stresses and restraint.

Nowadays GTAW welding machines have Facility with PreFlow and Post flow of Shielding Gas which could be of one option and second option is to use correct Bead size while starting and finishing not necessarily a Key Hole Technique to be followed.

Thanks & Regards

J.Gerald Jayakumar

0091-9344954677



On Wednesday, November 1, 2017, 12:29:43 AM GMT+4, PGoswami <pgoswami@quickclic.net> wrote:


Hi Amul,

 

These cracks are  Centreline or Hot Cracks .I've attached a picture of the same from the book. The contributing factors could be :-

 

1.       Technique wise

·         Too fast or Jerky removal of the filler metal from the weld puddle, gradual or slow removal of the filler from the weld puddle  may help sometimes.

 

2.       Filler metallurgy wise:

·         check what's the ferrite no for the weld deposit. Typically for 347 H one would require 6 TO 8FN or more in the deposit to avoid cracks.

·         Check what's the Nb:C ratio. It should be 8 Max. Higher values(i.e. more Nb in the weld) could contribute to cracking.

 

3.       Filler Batch/ Box Specific:

·         Try welding with filler from another  box or batch no, see if it helps

 

I'll look forward to your response.

 

Thanks.

 

 

P.Goswami.P.Eng, IWE.

Welding & Metallurgical Specialist

Linkedin: https://www.linkedin.com/in/pradip-goswami-2999855/

Email:pgoswami@quickclic.net,pradip.goswami@gmail.com

 

 

 

Fig.3. Buried centreline cracking

Fig.3. Buried centreline crackiFig.3. Buried centreline cracking Fig.3. Buried centreline cracking ngFig.3. Buried centreline crackingFig.3. Buried centreline cracking

Fig.3. Buried centreline cracking

 

 

From: Amul Raj [mailto:win.amul@gmail.com]
Sent: October 31, 2017 8:35 AM
To: Pgoswami@quickclic.net; pradip.goswami@gmail.com
Subject: Heater coil welding getting Crack - Reg

 

Dear Sir, Good evening.....! 

 

In our project hydro cracker unit, Heater radial coil welding base material 347H and filler material ER347H(Metrode), size 4" X 13.49 Thick 

 

When we do the welding, getting Crack in the weld start and stop point 

 

Please advise me sir

 

Thanks and Warm Regards 

 

Amul Raj T  

PSCJV 

+965-66310230


Virus-free. www.avg.com

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...