Skip to main content

Re: [MW:25623] GMAW for CS

Reasons for pores could be plenty. It could be  due to

1. in adequate shielding - increase shielding gas flow rate to 12 to 15 lpm depends upon transfer mode.
2. Excessive shielding gas flow rate -  reduce gas flow rate if it is 25 lpm and above as it creating vacuum   
3. There could be leaks in between - Check with soap water solution. Tighten the clips properly.
4. Thee could be drought due to high velocity breeze while welding in open.
5. It could be also due to a higher stick out for amp / volt selection. 
    Average 15 &  max. 25 mm., depending up on transfer mode 
6. Argon with 18 /20 CO2 will be good for CS. Pure Argon may induce undercuts.

Sridhar.


From: George Dilintas <dilintas@gmail.com>
To: Meghanadh K <materials-welding@googlegroups.com>
Sent: Friday, 7 October 2016 1:35 PM
Subject: Re: [MW:25503] GMAW for CS

arc stability issue

2016-10-04 13:01 GMT+03:00 Kannayeram Gnanapandithan <kgpandithan@gmail.com>:
Do not use Pure Argon, Mix with Oxidising gas like O2 or CO2

THANKS & BEST REGARDS,
KG.PANDITHAN, IWE,  AWS-CWI, CSWIP 3.1,
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349

On Mon, Oct 3, 2016 at 2:15 PM, 'MAGHROUD Moussa' via Materials & Welding <materials-welding@ googlegroups.com> wrote:
Boxbe This message is eligible for Automatic Cleanup! (materials-welding@googlegroup s.com) Add cleanup rule | More info



Dear experts

I am trying to qualify a PQR using GMAW applied on a plate spec A36,10 mm thick, ER 70S6 1.2 mm, position 3G, progression downhill and Argon pure as shielding gas. But after RT shooting we find porosity throughout the joint. 
Please anyone can help how to qualify this weld. 


Envoyé depuis un mobile Samsung
--
http://www.linkedin.com/groups /MaterialsWelding-122787?home= &gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@ googlegroups.com.
To post to this group, send email to materials-welding@googlegroups .com.
To view this discussion on the web visit https://groups.google.com/d/ms gid/materials-welding/75mxu7h0 eetcco1lxwgeo5h9.1475484008276 %40email.android.com.
For more options, visit https://groups.google.com/d/op tout.


--
http://www.linkedin.com/ groups/MaterialsWelding- 122787?home=&gid=122787&trk= anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@ googlegroups.com.
To post to this group, send email to materials-welding@ googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/ msgid/materials-welding/ CAJzm4eO2FRye_ gZwLfPXkgczC0qDxay7uZhg9JgVbtj y3cN7PQ%40mail.gmail.com.
For more options, visit https://groups.google.com/d/ optout.



--
Dr. Georgios Dilintas,
Dipl. Ing. In Aeronautic and Space Engineering
Ph.D in Mechanics of Solids - Computational Mechanics
A.I.S, A.N.I, IRCA Lead Auditor
Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAPOi40DLzs74%3DGtw1J1-g24zE7rSziW6M5wga_oM4HFaE4fqAA%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.


Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...