Use a TGX filler metal ( this a flux core filler wire) make a slag blanket which it's denesity is higher than ofthe denesity of molted metal ;this way enable us to protect root from oxidizing. Don't forget use low heat input.

On 3 Dec 2014 10:04, "Pravin Poornachandran" <htcispravin@gmail.com> wrote:
Dear Sir,


In such situation, base on my experience in welding, you can use special filler rod to perform such welding.

In KOBELCO welding consumable, TG-X316L, TG-X308L can be use to weld such application because
these consumable doesn't require back purging during welding.

Special chemical elements is added into this filler rod which can act as oxidation agent.

Attached is the technical literature of KOBELCO TG-X series.

Kindly refer to the attachments.

P.S: This filler rod can be only used for root pass only, balance pass continue to use SMAW or FCAW.

Best regards,
Pravin Poornachandran
Singapore

On Tue, Dec 2, 2014 at 11:01 PM, S.Mohammed <mohd52100@gmail.com> wrote:

Dear all,

How  i can repair SS 316L/304L sch 40 thk field weld where it is difficult/not economical (line very long) to purging?
Process :GTAW.

Regards,

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...