Re: [MW:19953] Welding consumable for cladded plate SA516 Gr70 with SS316

Dear Ramon
Sorry to say but your above providing information is not completely true.
i don't have t knowledge of piping welds but have well knowledge of ASME Sec VIII Div 1
as per UCS-56 you shall apply PWHT for a butt welds of more than 32 mm thickness ( if preheat is less than 95 Deg ) or more than 38 mm in any case . also all the butt welds shall be 100% radio-graphed for CS materials if thk exceed 32 mm as per UCS-57.

Thanks
Regards
Intekhab Alam Ansari



On Fri, Jan 24, 2014 at 7:13 AM, ramón ignacio briceño <bricenori@hotmail.com> wrote:
Dear Thuan,

All CS equipment fabricated by welding  following a PWHT after the welding if the base material thickness is more than 25 mm by plate or 19 mm by  piping.  ASME Section VIII-UG Part give you information about the form that you can apply the PWHT.

Regards, 
Ramon Briceno
Metallurgicla Engineer.

Subject: RE: [MW:19912] Welding consumable for cladded plate SA516 Gr70 with SS316
Date: Thu, 23 Jan 2014 13:09:43 +0700


Dear Ramon Briceno,

 

Thank you so much for your information,

Yes, the ER-309 is intersection between CS Vs SS then after ER-316L for cladding..

How about PWHT for thickness over 30mm CS?

 

 

Regards,

Thuan, Vu Duc

Mobil: +84 983 017 936

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of ramón ignacio briceño
Sent: Thursday, January 23, 2014 8:32 AM
To: materials
Subject: RE: [MW:19908] Welding consumable for cladded plate SA516 Gr70 with SS316

 

Dear Thuan,

According your requirement of cladding SA516-70 / SS316, begin the work  of "buttering"  with ER-309 filler to facilitate the microstructural transition between CS vs SS. This "buttering" can be 1 mm thickness and following use ER-316L filler to end  up with 2 mm thickness. Use SMAW process, and depending of the cladding area to cover, change the aplication by SAW process, then you need a other welding material of common use in SAW process to joint  SA516-70 / SS316L.

 

Regards, 

Ramon Briceno

Metallurgical Engineer.

 

  


From: dthuan117@gmail.com
To: materials-welding@googlegroups.com
Subject: [MW:19902] Welding consumable for cladded plate SA516 Gr70 with SS316
Date: Wed, 22 Jan 2014 12:10:55 +0700

Dear Expert ,

We have vessel shell plate A516-Gr 70 cladded with SS316 L, For the plate thickness: 25MM-40MM cladded 3mm.

Could you please advise the filler material selection and welding sequence for LS and CS.

I intend to use welding process FCAW and SAW. Or SMAW and SAW.

 

Thanks and Best regards,

 

 

 

Regards,

Thuan, Vu Duc

Mobil: +84 983 017 936


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

Comments

Popular posts from this blog

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

[MW:5202] RE: 5200] NDT after PWHT

------------------------------------- Interpretation:  I‑89‑14 Subject:         Section I (1986 Edition, 1987 Addenda), PW‑11,                  NDE Prior to PWHT Date Issued:     December 15, 1988 File:            BC88‑393   Question: Does PW‑11 require that NDE be performed on welds after they have been subjected to the postweld heat treatment required by PW‑39?   Reply: No, unless the conditions described in PW‑11.2.2 exist. ---------------------------------------------- Interpretation:  VIII-1-98-09 Subject:         Section VIII, Division 1 (1995 Edition, 1996 Addenda); NDE                 ...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...