Monday, October 14, 2013

Re: [MW:18944] Tandem SAW for SA 240 Type 304 100mm thick

Dear Hrushikesh:

Hot cracking should not be your main concern but impact test might cause you problems.
I had an experience with 304L (67mm) plate and we used 3.2mm wire (single arc SAW) and we were checking interpass temperature regularly.

In tensile test, elongation did not reach min requirement.
Our impact test was at -120 deg.C and almost all specimens, had a shear type fracture surface with very low lateral expansion (rejected). Impact tougness were mostly between 28 and 40 J.

If you use tandem arc, heat input will be higher and you may face problems.
Of course we were using K-configuration for our joint and yours is J-configuration which is much better.

I do not recommend you tandem arc unless you use small diameter wires (1.6mm) in which heat input is not much different than that of single arc with larger dia wires (2.4mm). So my recommendation is to use single arc. Keep interpass temperature as low as possible (even cooling with water etc.).

Regards
Ramin Kondori
Sr. QA/QC Engineer
SINOPEC

r.kondori@petroyada.com
+98-2123592322
+98-9132150320



On Sat, Oct 12, 2013 at 6:58 PM, Hrushikesh Sangamnerkar <hrushi612@gmail.com> wrote:
Dear all,

Base Material: SA 240 Type 304/304L
Filler Metal : SFA 5.9 ER 308/308L (2.4mm/3.15mm dia)
Joint Design: "J" groove
Root face : 5mm
Back chip is allowed.

I am in process to qualify PQR for Tandem SAW. 

Since thermal conductivity of SS is low. 
1) What precautions are required to be taken while caring out Tandem SAW specially for SS.
2) Are there chances of solidification cracking? If yes, what can be the possible reasons and precautions to be taken.
3) Does thermal conductivity have any role to play with cracking?

Kindly provide your suggestions.

Awaiting the reply.

Thanks and regards,

Hrushikesh H Sangamnerkar
09724738118

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

No comments:

[MW:34920] Tubesheet Hole step

Hello Team, I have one question any tolerance given for tubesheet Hole step. Please do needful. Regards, AP  -- https://materials-...