ER Ni Cu - 8 ( with 70 Ni & 30 Cu) could be used for welding Cupronickel (Cu Ni) to carbon steel.
Sulfur & Phosphorous should be kept at max. of 0.02% and with absence of Pb and additions of Mn .
will help to get crack free joints
From: prabhu <prabhujeetnikam@gmail.com>
To: materials-welding@googlegroups.com
Sent: Wednesday, 9 October 2013 9:08 AM
Subject: [MW:18886] Welding of CuNi 70/30 to SA106
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
Sulfur & Phosphorous should be kept at max. of 0.02% and with absence of Pb and additions of Mn .
will help to get crack free joints
From: prabhu <prabhujeetnikam@gmail.com>
To: materials-welding@googlegroups.com
Sent: Wednesday, 9 October 2013 9:08 AM
Subject: [MW:18886] Welding of CuNi 70/30 to SA106
Dear All,
-- Can anyone tell me which filler should be used for welding CuNi 70/30 to SA106. by using GTAW process.
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
No comments:
Post a Comment