Hello Abhisekh Rai,
 
What's the thickness involved here ??
 
Thanks
 
Pradip Goswami, P.Eng,IWE
Welding & Metallurgical Specialist
Ontario, Canada
 
 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of HAREESH K V
Sent: Monday, October 07, 2013 3:26 AM
To: materials-welding
Subject: Re: [MW:18867] PWHT Requirement for dissimilar welding b/w P91 & SS304


Sa335 Gr P91 side to be buttered up to a minimum of 13mm with ERNiCr-3. Then PWHT to be done for that side as per the requirement of P91 to P91 welding (Normally 720 deg temperature up to a minimim of 2hrs). Then face prepration is to be done (Ensure a 13mm buttering after this face prepration)

Then prepare the joint b/w P91 and SS304 and weld with ERNiCr-3

No PWHT requirements after this




On Sun, Oct 6, 2013 at 2:05 AM, Octane Mac <octane.mac@gmail.com> wrote:
B31.3: 704-760 C, minimum holding time 2 hrs. Holding time 1hr/in.
B31.1: 730-775 C, minimum holding time 30 minutes. Holding time 1hr/in. Note: As it is a dissimilar material welding and a nickel based consumable is recommended therefore minimum holding temperature shall be 700 C.

Octane



On Fri, Oct 4, 2013 at 7:33 PM, Abhishek Rai <abhishekkrrai@gmail.com> wrote:
Dear Sir,

Please confirm the requirement of PWHT b/w welding of P91 & SS 304.the operating temperature of piping is 640 deg c .

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.



--
----------------------
Hareesh K V
+91-9447625012


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

No comments:

[MW:34919] Welder qualification certificate

Dear All     anyone can share a format for welder certificate and card format        Thanks & Best Regards Saleem manhappulath Mob:+9665...