Re: [MW:18805] Impact testing failed with ER70S2 wire at -48°C & -35°C

 
Dear Mr. Prasad,
Please find my point wise reply
Aly
 
 
-------Original Message-------
 
Date: 9/27/2013 8:36:20 PM
Subject: Re: [MW:18784] Impact testing failed with ER70S2 wire at -48°C & -35°C
 

Hi,
 
provide me the follwoing details
 
1. With PWHT or without PWHT
With PWHT 650 deg C 180min
 
2. Size of Impact test coupon
10 x 10 x 55
 
3. Location of notch  ( weld center line, HAZ ( FL or FL+1 or FL+2 )
WCL & HAZ
WCL failed and HAZ passed
 
4. Base metal details  
SA516 Gr65 to SA516 Gr70
 
5. Test coupon size 
 
50mm test coupon
19mm SMAW with E7018-1 top side ,
12mm GTAW with ER70S2 middle and
19mm SAW with F7P10 EH12K bottom
 
 
Regards
 
N.V. PRASAD
 
 
 
On Sun, Sep 22, 2013 at 1:00 PM, Mhaskar Aly <mhaskar.aly@gmail.com> wrote:

Dear Friends,

 

I have tested one PQR where Impact testing (GTAW weld) got failed at -48°C & -35°C also;
 
Impact values
9 joules at -48°C
12 Joules at -35°C
 
 
I had received Filler wire with 3.1 certificate having impact tested at-50°C; kindly advise

 

Heat Input max

2.58KJ/mm Root run &

1.8Kj/mm for other runs
 
Kindly advise
 
Ali Mhaskar

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...