Dear ,

Where it is mentioned Base metal thick to be considered??

Example:

your thickness is 8mm means width across the notch is less than 80% so you prefer to have subsized 5mm

New sub sized is ==10x5x55
Required sized is ==10x10x55

now temperature reduction is == -20-11.1== -31.1C and

Charpy energy if Original was 27J then new one as per A370 table-9 is 14J.

Hope this will clear.!!


On Saturday, August 17, 2013 11:35:48 AM UTC+3, nguyen tuan wrote:

Dear Experts

 

I have question about using sub-sized specimen for CVN test

Testing temperature following specification   is -20oc ,Plate thickness is 8mm and specimen sized is 10x5

My question How much temperature will apply for testing (AWS D1.1)

 

"4.36.7 When sub-sized specimens are required, and the

width of the specimen across the notch is less than 80%

of the base metal thickness, the test temperature shall be

reduced in conformance with Table 4.15, unless otherwise

specified in the contract documents

Thanks in advance

 

 

Tuan

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...