Hi Mohamed,

The same problem happened to us in other material, if problems in weld metal then let you check this PMI test on the weld metal after surface clean by wire brush (try equivalent filler metal type) and/or remove some weld metal then you may get right result.

if failed the above method, in this worst case let us assume up to which level did not get result so remove weld metal like gauge/scoop and check by PMI, if you got the result, that much you have remove weld metal from joints & re-weld its better way
Instead of cut out the full weld joint,

I hope this issue in surface level only,

Best regards,
Bala. R
+7 906 459 2882
 
On Thu, Aug 30, 2012 at 2:40 PM, pgoswami <pgoswami@quickclic.net> wrote:
Mohamed,
 
The results are surprising.
 
D&H Secheron manufactures welding consumables of extremely good quality. I 'm going back to  the days of late 1980s  and early 1990s.  Usually they stand behind their quality. Are you sure there's no mix up of welding consumables during the field or shop fabrication?
 
You may run a test pad  for all weld deposit conforming to ASME Sec-II Part C, SFA 5.28 any see how it differs to the consumable MTR. This could be done by XRF.If the consumable test pad conforms to Grade -91 ( ER 90S-B9 filler metal) then certainly it's mix up during welding.
 
Another way is that scoop up some amount of weld metal and perform a wet/lab analysis and see what're  the results.
 
Let's know if it helps.
 
Thanks.
 

Pradip Goswami,P.Eng.IWE

Welding & Metallurgical Specialist

Ontario, Canada.

Email-pgoswami@sympatico.ca,

pgoswami@quickclic.net

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of mohamed jubair
Sent: Tuesday, August 28, 2012 3:25 AM
To: materials-welding@googlegroups.com
Subject: [MW:15142] Problem about Positive material Identification(PMI)

 


Dear all,

 

In our  boiler one major problem occurred in Positive Material Identification(PMI) test [Spectrum test].  

 

Description

Reheater finishing outlet(RHFO) coil

Material

T91

Size

ø 63 x 4

Process

GTAW only

Filler wire

ER 90S B9

Filler wire Manufacturer

D & H Secheron

Preheating °C

185

Rate of Heating  °C

100/hr

Interpass temp  °C

190

Post heating  °C

100

PWHT  °C

750

Soaking Time

90 minutes

 

Around 800 joints welded in the above approved procedure only. Filler wire, header stub, RHFO coil, weld metal undergone PMI test separately and all show positive material results as T91 except weld metal. Weld metal shows the Chromium content only  as (4-7%){Reqd is 8-10.5%}.  We can't find how it happened? Our Chinese consultant told to cut and reweld all the joints. But our contractor argued that we followed approved procedure and used approved vendor's consumable only. Please give a solution. Here I have attached one preheating cum PWHT chart of RHFO joints(for 11 joints,5 thermocouples,1 recorder).All 800 joints are not checked yet. Only 40 joints checked and all 40 weld metals shown low Cr Content.

 

Please go through the below readings of one RHFO joint.

Description

Filler wire

Header stub

Weld metal

RHFO coil

 Alloy

T91

T91

A-2

T91

Cr

8.94

8.34

5.19

8.68

Mo

0.96

0.90

0.93

0.92

V

0.17

0.17

0.08

0.19

Ti

0.07

0.10

0.04

0.03

Mn

0.60

0.40

0.54

0.63

Fe

87.81

88.11

90.86

87.61

Ni

0.12

0.33

0.20

0.38

Cu

0.02

0.16

0.20

0.16

Nb

0.09

0.08

0.03

0.04

W

0.15

 

0.00

 

 

Waiting for your valuable suggestions.

 

Thanks & Regards

K Mohamed Jubair

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 


______________________________________________________________________
The information in this email is confidential, and is intended solely for the addressee(s). If you are not the intended recipient of this email please let us know by reply and then delete it from your system; you should not copy this message or disclose its contents to anyone. The internet can not guarantee the integrity of this message. HAMON (and its subsidiaries) shall (will) not therefore be liable for the message if modified.
______________________________________________________________________

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...