Hi,
If your vessel under service requirement, you should do PWHT after repair.
If it is not under service requirements, then you can do repair to increase the fillet size without PWHT but repair should be done before hydrostatic test.
Please refer UCS56(f).
Thanks & Regards,
(Karthik)
Karthikeyan.S
QA/QC Manager
German-Thai Boiler Engineering Cooperation Limited.
Rayong Factory ;
379 Moo.6 Soi 8, Tambol Pananikom,
Nikompattana, Rayong 21180 THAILAND
Tel : +66 38 897 035-9 Ext. 137
Fax : +66 38 897 034
Hand Phone: 0066 892512282
From: asad azmi <azmiasadayub@gmail.com>
To: materials-welding@googlegroups.com
Sent: Saturday, August 11, 2012 4:45 AM
Subject: [MW:15058] PWHT REQUIREMENT FOR REPAIR OF FILLET WELD
Dear All,
Greetings.
A Vessel is being fabricated as per ASME SEC VIII DIV 1.
Material of the Shell is SA 516 GR 70 HIC - 30 mm Thk.
PWHT of the vessel is already completed. PWHT is a Service requirement.
After PWHT it was found out that FILLET WELD of NOZZLE PAD to SHELL is less than the requiremnt. Nozzle Pad thickness is 30 mm. pad is welded on external surface of the shell.
Actual fillet is 12 mm less than the required fillet size.
Please advice whether Repair ( increase of fillet weld size) can be done without RE- PWHT.
Please give Code reference.
Thanks & Regards
Asad Azmi
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
Comments