[MW:15142] Problem about Positive material Identification(PMI)


Dear all,

 

In our  boiler one major problem occurred in Positive Material Identification(PMI) test [Spectrum test].  

 

Description

Reheater finishing outlet(RHFO) coil

Material

T91

Size

ø 63 x 4

Process

GTAW only

Filler wire

ER 90S B9

Filler wire Manufacturer

D & H Secheron

Preheating °C

185

Rate of Heating  °C

100/hr

Interpass temp  °C

190

Post heating  °C

100

PWHT  °C

750

Soaking Time

90 minutes

 

Around 800 joints welded in the above approved procedure only. Filler wire, header stub, RHFO coil, weld metal undergone PMI test separately and all show positive material results as T91 except weld metal. Weld metal shows the Chromium content only  as (4-7%){Reqd is 8-10.5%}.  We can't find how it happened? Our Chinese consultant told to cut and reweld all the joints. But our contractor argued that we followed approved procedure and used approved vendor's consumable only. Please give a solution. Here I have attached one preheating cum PWHT chart of RHFO joints(for 11 joints,5 thermocouples,1 recorder).All 800 joints are not checked yet. Only 40 joints checked and all 40 weld metals shown low Cr Content.


Please go through the below readings of one RHFO joint.

Description

Filler wire

Header stub

Weld metal

RHFO coil

 Alloy

T91

T91

A-2

T91

Cr

8.94

8.34

5.19

8.68

Mo

0.96

0.90

0.93

0.92

V

0.17

0.17

0.08

0.19

Ti

0.07

0.10

0.04

0.03

Mn

0.60

0.40

0.54

0.63

Fe

87.81

88.11

90.86

87.61

Ni

0.12

0.33

0.20

0.38

Cu

0.02

0.16

0.20

0.16

Nb

0.09

0.08

0.03

0.04

W

0.15

 

0.00

 

 

Waiting for your valuable suggestions.

Thanks & Regards
K Mohamed Jubair

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...