Re: [MW:14803] Filler Materail required for welding SS 321 to SA 516 gr-70

Hi

It depends on working temperature of your equipment, If temperature is above 315°C you have to use ER309L as a buttering pass and ER321 for filling passes, you can use welding handbook(dissimilar welding section) and API 582 as a reference.

Regards,
Himan

 


On Sat, Jul 7, 2012 at 8:30 PM, <osikwemhepaul@gmail.com> wrote:
Hello Ankit
Use ER309L

Sent from my iPad

On 07 Jul 2012, at 1:20 PM, "Ankit Patel" <ankit.patel@orientalindia.net> wrote:

Dear Experts,

 

I want to weld SA 516 GR-70 plate to SA 182 TP 321.

 

Kindly suggest me the filler material grade used  for welding this material.

 

Thanks & Regards

Ankit Patel
Engineer Quality

 

<image001.jpg>

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:34919] Welder qualification certificate

Dear All     anyone can share a format for welder certificate and card format        Thanks & Best Regards Saleem manhappulath Mob:+9665...