Hi
 
The tapered burning of electrode is due to its eccentricity problem which is a manufacturing problem caused during extrusion process of electrode.
Please replace the defective electrodes with a new Batch.
If you weld with eccentric electrodes you might land up in defects in UT/RT.
 
Regards
 
Prem Nautiyal

--- On Thu, 7/5/12, Materials & Welding <materials-welding@googlegroups.com> wrote:

From: Materials & Welding <materials-welding@googlegroups.com>
Subject: [MW:14767] Tapered burning of MMA electrode
To: materials-welding@googlegroups.com
Date: Thursday, July 5, 2012, 12:14 PM

Dear Experts
I am Facing a problem in SS 308-16 MMA electrode diameter 2.5 mm 
when I start welding It gives tapered burning of electrode
what can be the possible reasons from welding point of view and electrode manufacturing point of view???
How this problem can be solved?

Regards,
Ahmed
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:34919] Welder qualification certificate

Dear All     anyone can share a format for welder certificate and card format        Thanks & Best Regards Saleem manhappulath Mob:+9665...