RE: [MW:12557] Uncontrolled heating and cooling effect of Carbon steel below lower critical temperature

Limesh

 

Simple rule:  you will have no phase changes unless the steel is heated above the lower critical temperature (LCT). 

 

If you have an alloy steel, the lower critical temperature will be different than for a carbon steel, but the above rule applies.

 

If the maximum temperature is below the lower critical, there will be no phase change but coarsening of pearlite will occur.  Other structural changes may occur but the phases will not be effected (creation of tempered martensite or bainite, redistribution of stresses, creep due to stress relief etc.). 

 

The major reason heating and cooling rates are restricted are to prevent the creation of residual stresses usually caused by uneven distribution of heating/heat removal .  These stresses can cause cracking, particularly in highly restrained structures.

 

{Note with regard to the simple rule above,  there will be an apparent upward shift in LCT with increasing heating rate (diffusion controlled process) with respect to the equilibrium LCT.  Similarly, there will be an apparent downward shift in the upper critical temperature (UCT) for diffusion dependent processes with respect to the equilibrium UCT.}

 

Any further questions, please append.

 

John A. Henning

Senior Engineer, Welding & Materials

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of limesh M
Sent: Monday, September 26, 2011 1:59 AM
To: materials-welding@googlegroups.com
Subject: Re: [MW:12534] Uncontrolled heating and cooling effect of Carbon steel below lower critical temperature

 

Mr. Muthu Bharathy,

These phenomena has already been proved well before by scientists.These things are well explained by authors like Sidney H. Avner,George E. Dieter,Sir Allen Cottrel,William D. Callister,Herman W.Pollack etc. in their material science and metallurgy books.Because Austenite is the one plays a major role to form other phases or micro structure during cooling(Cooling rate has great significance in getting coarse or fine grained micro structure).For example,without austenite ,there is no martensite formation in carbon steel during rapid cooling(quenching) from above upper transformation temperature due to lattice shear(no time for diffusion) and I don't think that martensite simply exists as it is.These phenomena is well explained in CCT and TTT diagrams.If you have any different opinion or my understanding is wrong ,you are most welcome to explain it as I don't have much expertise in material science.Moreover, my query was about the phase changes with in the limit of lower critical temperature of Iron-Iron carbon equilibrium diagram during uncontrolled heating and cooling.

Furthermore,I didn't get what do you mean by 'prove' since I didn't claim any kind of invention in my query!!

Regards,

Limesh

On Sun, Sep 25, 2011 at 2:41 PM, muthu barathi <muthu_barathi@rediffmail.com> wrote:



Dear Sir,


Better you may make a trial experiment and prove it.


Thanking You,

Honesty is the best Policy

With Warm Regards,

Muthu Barathi P
Mobile No:00962788269821 (Jordan)
00962775401951


From: limesh M <limesh78@gmail.com>
Sent: Sun, 25 Sep 2011 12:53:25
To: materials-welding@googlegroups.com
Subject: Re: [MW:12515] Uncontrolled heating and cooling effect of Carbon steel below lower critical temperature


Dear Mr. Biplab,

As per my understanding,TTT (C-Curve)or CCT won't give any idea on my query.Both diagrams discussing about the phase changes occurs on cooling above upper transformation temperature.So,CCT or TTT gives information on austenite decomposition.For a hypothetical manner we can say above lower critical temperature on hypo-eutectoid steel as it contains partial gamma iron(austenite) and alpha iron(ferrite).

Regards,

Limesh


On Mon, Aug 22, 2011 at 4:12 PM, Biplab Pal <biplab.mech@googlemail.com> wrote:

You should go through TTT diagram.

On Sun, Aug 21, 2011 at 7:48 PM, limesh M <limesh78@gmail.com> wrote:

Dear All,



Material : Carbon steels in between 0.008% carbon and 6.67 % carbon.

1.Is there any metallurgical changes(phase change) will occur other than pearlite,if I heat rapidly uncontrolled heating)low carbon steel just below or equal to lower critical temperature(723 C) as per iron-carbon equilibrium diagram?

2.1.Is there any metallurgical changes(phase change) will occur other than pearlite,if I cool rapidly (uncontrolled cooling, no quenching by any kind of liquid medium)low carbon steel from just below or equal to lower critical temperature(723 C) as per iron-carbon equilibrium diagram?





Regards,

Limesh

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.




--

Thanks & Regards

Biplab Pal
Industrial Services, Inspection Engineer.
SGS India Pvt. Ltd.
Kolkata Branch

E-mail:   biplab.mech@gmail.com
 
Information in this email and any attachments is confidential and intended solely for the use of the individual(s) to whom it is addressed or otherwise directed. Please note that any views or opinions presented in this email are solely those of the author and do not necessarily represent those of the Company. Finally, the recipient should check this email and any attachments for the presence of viruses. Myself accepts no liability for any damage caused by any virus transmitted by this email.

 

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Error! Filename not specified.
Treat yourself at a restaurant, spa, resort and much more with Rediff Deal ho jaye!

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

The Schaeffler and Delong diagrams for predicting ferrite levels in austenitic stainless steel welds

Introduction Ferrite is important in avoiding hot cracking in during cooling from welding of austenitic stainless steels. 'Constitution diagrams' are used to predict ferrite levels from the composition by comparing the effects of austenite and ferrite stabilising elements. The Schaeffler and Delong diagrams are the original methods of predicting the phase balances in austenitic stainless steel welds. Nickel and chromium equivalents A 'nickel equivalent' is calculated for the austenite stabilising elements and a 'chromium equivalent' ferrite stabilising elements. These are used as the axes for the diagrams, which show the compositional equivalent areas where the phases austenite, ferrite, martensite (and mixtures of these) should be present. Although intended to show the phase balance of weld fillers, these diagrams can also be used to illustrate the phase balance of the 'parent' material. There are different diagrams for dif...