Re: [MW:12526] WPS Heat treatment condition

Hi,
Change in PWHT Tine and Temperature range is a supplementary essential variable. If there is no Impact requirements,you can use your existing WPS. If there is any Impact test required , QW 407.2 applicable.

QW-407.2 A change in the postweld heat treatment

(see QW-407.1) temperature and time range

The procedure qualification test shall be subjected to

PWHT essentially equivalent to that encountered in the

fabrication of production welds, including at least 80% of

the aggregate times at temperature(s). The PWHT total

time(s) at temperature(s) may be applied in one heating

cycle.

QW-407.6 A change in postweld heat treatment condition

in QW-407.1 or an increase of 25% or more in total

time at postweld heat treating temperature.


Thanks & Regards,

(Karthik)

Karthikeyan.S
QA/QC Manager
Getabec Energy Co.,Ltd.
379,Moo6,Soi8,Nikhomphatana,
Rayong-21180,
Thailand.
Phone: 0066 38 897035-8 (Off)
Fax: 0066 38 897034
Hand Phone: 0066 892512282


--- On Sun, 9/25/11, muthu barathi <muthu_barathi@rediffmail.com> wrote:

From: muthu barathi <muthu_barathi@rediffmail.com>
Subject: Re: [MW:12519] WPS Heat treatment condition
To: "materials-welding@googlegroups.com" <materials-welding@googlegroups.com>
Date: Sunday, September 25, 2011, 4:14 PM



Dear Sir,

You may check your existing PQR soaking temperature tolerance. Normally we will give +/- 40 to 50 degree Celsius. If it is with in that range you may use the same one.



Thanking You,

Honesty is the best Policy

With Warm Regards,

Muthu Barathi P
Mobile No:00962788269821 (Jordan)
00962775401951


From: Vijay Katkar <katkar.vijay22@gmail.com>
Sent: Sun, 25 Sep 2011 12:54:36
To: materials-welding@googlegroups.com
Subject: [MW:12516] WPS Heat treatment condition
Dear All,
Regarding heat treatment ,
I have P1 to P8 PQR with following heat treatment,
 
Loading temperature :- 350  ĢŠC
heating rate : 70   ̊C  /hr
Socking temperature: 620  ̊C
Cooling rate : 70  ̊C/hr
Unloading temperature: 350  ̊C
 
our job requirement is
Loading temperature :- 350  ̊C
heating rate : 70  ̊C/hr
Socking temperature: 670  ̊C
Cooling rate : 70  ̊C/hr
Unloading temperature: 350  ̊C
 
Is it possible to use above PQR for same job if yes please tell me the reference in section IX. or this not possible then why because above all temperature below lower critical temperature..
please advice your valuable experience..............
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


Treat yourself at a restaurant, spa, resort and much more with Rediff Deal ho jaye!
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...

Re: [MW:10788] ON PLOT PIPING & OFF PLOT PIPING

Piping systems involved for the flow lines and gathering lines from the well head isolation valve to the production facility or processing plant isolation valve are determined as OFF PLOT. ON PLOT defines piping system in the processing plant and production platform. ANSI/ASME B31.4 applies for off plot piping system. B31.4 allows the use of either API 1104 or ASME section IX (as appropriate). However, occasionally, a very small system such as piping within 500 feet of a processing plant (some client also said 400 feet) may be declared B31.3 rather than B31.4. When B31.3 is invoked, only ASME Section IX is used. before you decide which code to use for welding procedure and/or welder qualification for pipe welding, you have to know the design and construction code applicable to the system. Please read far enough into scope and diagram illustrating the application of either B31.3 and B31.4 hope this helps rgds 2011/4/21 pradip kumar sil < pradipsil@gmail.com > Dear all, ...