Re: [MW:12264] If Dia of Filler Rod changes what would be Volts , Amps & Travel Speed

you have to maintain heat input,

as heat input = voltage * current / travel speed

regards

dinesh

On Thu, Aug 18, 2011 at 4:58 AM, Abraham <QIS-009@hdec.co.kr> wrote:

Dear all

 

I need to make a WPS as per ASME SEC IX & Construction Code is ASME B31.3

 

PQR :  12" 42 THK 

Material :  SA335 P22

Process :  GTAW + SMAW

 

Actual Filler Wire Used in PQR  : 3.2 mm  Dia Rod  ( Amps : 100 ~ 125  , Volts : 23 ~ 26 , Travel Speed : 10 ~ 15 Cm / Min )

 

But in our site we are using 2.4mmm , 3.2 mm , 4.0 mm Dia Filler Rods

 

I want to make a WPS mentioning Current , Volt  , Travel speed for this 2.4 mm & 4.0 mm Rod also .

 

What basis  and Which clause I can get consequent A , V & TS  ?  

 

 By below clause we can support our WPS but cant get the value for A , V & TS .

                                             

                                               (i) 404.3 Change in Size of Filler metal is Non Essential Variable

                                               (ii) 409.8 Change in I & E Range is an Non Essential Variable

                                               (iii ) 409.1  Heat input increase in Supplementary Essential Variable . My case no need Impact Testing

 

 

Thanks and Regards

 

A.P.Abraham ,

Qatar .

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

[MW:30043] Weep hole

If weep hole is not provided in dummy pipe before welding What will happen??? -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/da251ee6-fa7f-4851-b876-cdb3834ae341%40googlegroups.com .