Re: [MW:11417] SS 304L piping leaking

Is there any rust visible on the piping? If yes, the chances are the welders have mixed up filler metals at some point of time.
 
CSCC may be possible depending upon the salinity of water if there is any vibration caused by cyclic loading. Otherwise, the CSCC is less likely for Utility water service in such a short period.
 
Regards,
 
Prasad Joshi
 
On Mon, Jun 20, 2011 at 7:36 PM, Fred Majdnia <FMajdnia@technip.com> wrote:
   Dear Kumaran,
 
For a technical root cause analysis you need to perform the testing of the water. The dissolved gases, PH, chloride ion being the most important parameters. Without the water analysis report, no one can help and all would be guess and anticipation. 
I can guess the reason but prefer to leave it to the test result.
 
Regards
 
 
-----materials-welding@googlegroups.com wrote: -----

From: Raghuram Bathula <raghurambathula@gmail.com>
Sent by: materials-welding@googlegroups.com
Date: 06/19/2011 11:55PM
Subject: Re: [MW:11397] SS 304L piping leaking


it depends on salinity (ppm) and temperature also, any chance of mixng sea water?

On Mon, Jun 20, 2011 at 11:16 AM, k.ilangkumaran ilangkumaran <k.ilangkumaran@yahoo.com> wrote:
Dear experts,
 
                Could you please anyone explain me why SS 304L piping leaking. Its service is just utility water and duration of service is not even 1 year. Also leaks were observed many locations only on weld and HAZ. What could be the causes leak?
 
Regards
Ilangkumaran
 


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


    This email and any attached files ("Message") may contain confidential and/or privileged information. It is intended solely for the addressee(s). If you receive this Message in error, inform the sender by reply email, delete the Message and destroy any printed copy. Any unauthorized use, distribution, or copying of this Message or any part thereof is prohibited. Emails are susceptible to alteration. Neither Technip nor any of its affiliates shall be liable for the Message if altered or falsified nor shall they be liable for any damage caused by any virus that might be transmitted with this Message. 

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

Re: [MW:35289] Welding consumable for S355J2WP material

S355 J2 WP  is a weathering structural steel  It has better atmospheric corrosion resistance. Use E 8018 - W1/W2  Electrodes This is regular...