[MW:11266] RE: 11264] COMBINATION OF 2 PQR IN ONE WPS

No - if ASME Section IX is the governing Code.

See ASME Section IX QW-200.4 especially QW-200.4 (b).

QW-200.4 (b) allows combination of root procedure with any thicker
qualified fill procedure provided the base metal thickness as 13mm or
greater.

John

-----Original Message-----
From: materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] On Behalf Of manoj john
Sent: Monday, June 06, 2011 6:56 AM
To: materials-welding@googlegroups.com
Subject: [MW:11264] COMBINATION OF 2 PQR IN ONE WPS

Dear All,

I have to weld 40 mm thk ss 304 plate to be welded with root GTAW and
subsequent run by SMAW. I have 2 WPS,one WPS GTAW + SMAW thickness
range qualified is 1.6 to 12 mm and another procedure qualified 5 mm
to 50 mm with back gouging.

My doubt is can i make one wps supporting with these 2 Procedure
Root with GTAW and subsequent run with SMAW so i can carry out the
welding with GTA + SMAW 40 mm thk without further procedure
qualification.

Thanks & Regards.
Manoj

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to
materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views
and meant for educational purposes only, Users must take their own
decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

Re: [MW:35289] Welding consumable for S355J2WP material

S355 J2 WP  is a weathering structural steel  It has better atmospheric corrosion resistance. Use E 8018 - W1/W2  Electrodes This is regular...