Yes, Code gives the classified value without testing.
if you want higher, you need testing for the batch and confirmation.

arun

On Sun, Oct 24, 2010 at 3:32 PM, kannayeram gnanapandithan <kgpandithan@gmail.com> wrote:
pl check for 70S-3 only minus 20 celsius and 70S6--minus 30 celsius as per code.u have to test and confirm
kgp

On Sat, Oct 23, 2010 at 8:43 PM, Arunachalam A <arunvani@gmail.com> wrote:
SMAW:
Above   Minus 29 Deg C- E7018 ( This electrode is classified for above Minus 29 Deg C, means Mfrs give guarantee of impact property for that temp)
Above   Minus 46 Deg C -E7018-1 (This electrode is classified for above Minus 46 Deg C means Mfrs give guarantee of impact property for that temp )

GTAW:
Above  Minus 29 Deg C - ER 70 S-3 (This filler will give impact test values at Minus 29 Deg C )
Above  Minus 46 Deg C - ER 70 S-6 (This filler will give impact test values at Minus 46 Deg C because it has Managnrse content upto 1.85%

arun


On Sat, Oct 23, 2010 at 12:56 PM, SENTHIL P <senbe381@gmail.com> wrote:

DEARS,
WHAT ELECTRODES USED FOR LOW TEMPERATURE, WHAT IS THE REASON?




 EXPECTING URGENT REPLY

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
அருணாசலம்
கலைவாணி
சுதர்ஷனா
வருண்


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
அருணாசலம்
கலைவாணி
சுதர்ஷனா
வருண்


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:34920] Tubesheet Hole step

Hello Team, I have one question any tolerance given for tubesheet Hole step. Please do needful. Regards, AP  -- https://materials-...