Wednesday, October 9, 2013

RE: [MW:18883] PWHT Requirement for dissimilar welding b/w P91 & SS304

Hello Abhisekh Rai,
 
As explained by the other members , Buttering Grade-91(with Inconel -82/182) , performing PWHT , and thereafter welding SS304 would be the way to go. The welds between P-91 and SS 304 should subjected to PWHT as the last resort.
 
If there're many such dissimilar weld  joints and PWHT is the only solution then the attached  welding consumable could be a good option.(Note I'm not selling this product, acceptance is subject to vendor's interpretation).
This product was developed by EPRI & Metrode, see the detail in the attached documents. The only problem is it lacks AWS classification.
 
Hope this would be of help.
 
Thanks.
 
Pradip Goswami, P.Eng,IWE
Welding & Metallurgical Specialist
Ontario, Canada
 
 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Abhishek Rai
Sent: Monday, October 07, 2013 8:32 AM
To: pgoswami
Cc: materials-welding@googlegroups.com
Subject: Re: [MW:18870] PWHT Requirement for dissimilar welding b/w P91 & SS304

Dear Sir ,
the thickness of P91 material is 21 mm and for SS304 material is 12 mm. This is the fillet joint for support as running pipe is of P91 material and support pad is of SS304 H.
Please advise for PWHT & WPS .
Regard's
Abhishek Rai


On Mon, Oct 7, 2013 at 4:05 PM, pgoswami <pgoswami@quickclic.net> wrote:
Hello Abhisekh Rai,
 
What's the thickness involved here ??
 
Thanks
 
Pradip Goswami, P.Eng,IWE
Welding & Metallurgical Specialist
Ontario, Canada
 
 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of HAREESH K V
Sent: Monday, October 07, 2013 3:26 AM
To: materials-welding
Subject: Re: [MW:18867] PWHT Requirement for dissimilar welding b/w P91 & SS304


Sa335 Gr P91 side to be buttered up to a minimum of 13mm with ERNiCr-3. Then PWHT to be done for that side as per the requirement of P91 to P91 welding (Normally 720 deg temperature up to a minimim of 2hrs). Then face prepration is to be done (Ensure a 13mm buttering after this face prepration)

Then prepare the joint b/w P91 and SS304 and weld with ERNiCr-3

No PWHT requirements after this




On Sun, Oct 6, 2013 at 2:05 AM, Octane Mac <octane.mac@gmail.com> wrote:
B31.3: 704-760 C, minimum holding time 2 hrs. Holding time 1hr/in.
B31.1: 730-775 C, minimum holding time 30 minutes. Holding time 1hr/in. Note: As it is a dissimilar material welding and a nickel based consumable is recommended therefore minimum holding temperature shall be 700 C.

Octane



On Fri, Oct 4, 2013 at 7:33 PM, Abhishek Rai <abhishekkrrai@gmail.com> wrote:
Dear Sir,

Please confirm the requirement of PWHT b/w welding of P91 & SS 304.the operating temperature of piping is 640 deg c .

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.



--
----------------------
Hareesh K V
+91-9447625012


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.



--
Abhishek Kr.Rai
Engineers  India Limited

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

No comments:

[MW:34919] Welder qualification certificate

Dear All     anyone can share a format for welder certificate and card format        Thanks & Best Regards Saleem manhappulath Mob:+9665...