Hi Prasant,

Thermo-Mechanical Control Process (TMCP) is a  controlled rolling processes. TMCP produces fine-grained steel by a combination of chemical composition and integrated controls of manufacturing processes from slab reheating to post-rolling cooling. There are 2 variations:-

  1. Thermo-Mechanical Rolling (TMR):- fine grain size are produced by rolling in the recrystallization and the non-recrystallization regions of austenite, and sometimes in the dual-phase temperature region of austenite and ferrite. 
  2.  Accelerated Cooling (AC):- steels meeting the specified requirements are produced by promoting grain refinement and increasing the pearlite and/or bainite volume fraction through controlled cooling (accelerated cooling and air cooling) immediately after the final controlled rolling (CR) or TMR operation.
AR- stands for as rolled condition.Plate are heated above the AC3 temperature range and rolled in continuation ( either in a  single operation or multiple rolling cycles as required).Plates usually requires normalizing following rolling.
 
Pleas see the schematics below, which clearly outlines different processes. TMCP steels may be produced either by TMR or AC process, both producing  the similar steels with extremely high integrity
 
Pradip Goswami,P.Eng.IWE
Welding & Metallurgical Specialist & Consultant
Ontario,Canada.
Email-pgoswami@sympatico.ca,
 
 


From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of prashant pansare
Sent: Thursday, September 01, 2011 10:59 AM
To: mat wel
Subject: [MW:12330] process of AR-N & TMCP steel plates

Dear All,
What is the difference bet'n manufactring process of AR-N & TMCP steel plates?
Thanx & Regds,
PSP

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Re: [MW:34105] SA266 GR4N 4 Cycle SPWHT

Hi,  You are correct, Minimum refers to the one cycle for which this part will expose until final work shop PWHT. hence mill test certificate shall include this.  Max. SPWHT, refers to additional cycles of heat treatment that are reserved for future repairs during equipment lifetime.  Again, these simulated no. Of cycles shall be specified in MTC.  The idea is we need to make sure that steel mechanical properties are not compromised upon exposure to multiple repairs (i e 4 cycles in your case).  One could say, if steel is subjected to 4 cycles and is ok, then it should by defacto be good for one cycle, yet, this is wrong assumption cause mechanical problems and microstructure of materials varies accordingly based on no. Of cycles for which material will expose. This is apparent in alloy steel and especially for impact test values as an example.  In your case, this forged CS with properties before PWHT can be understood to be " as forged" condition (i.e. Wit...

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...