Dear Sujay,
QW-407.2 is applicable when impact test is required, it states that PWHT time mentioned in PQR shall be minimum 80% of what PWHT temperatue is goin to be used during Production Welding (at site or what is written in WPS).
Suppose I have PWHT 3 hours on the job. my PQR must have been qualified with PWHT time at least 180*80%=144 minutes. The recommended practice is to apply 2,5 times the PWHT time required for production to the PQR test coupons so that if in case you have to do repairs and repeat PWHT cycles, your PQR remains still valid. but make sure overheating doesn't affect mechanical properties.
Hope this would be helfull.
Regards
Manpreet Singh
On Wed, 19 Jan 2011 13:09:03 +0530 sujay kumarwrote
>
>To post to this group, send email to materials-welding@googlegroups.com
>To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
>For more options, visit this group's bolg at http://materials-welding.blogspot.com/
>The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
>
--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
QW-407.2 is applicable when impact test is required, it states that PWHT time mentioned in PQR shall be minimum 80% of what PWHT temperatue is goin to be used during Production Welding (at site or what is written in WPS).
Suppose I have PWHT 3 hours on the job. my PQR must have been qualified with PWHT time at least 180*80%=144 minutes. The recommended practice is to apply 2,5 times the PWHT time required for production to the PQR test coupons so that if in case you have to do repairs and repeat PWHT cycles, your PQR remains still valid. but make sure overheating doesn't affect mechanical properties.
Hope this would be helfull.
Regards
Manpreet Singh
On Wed, 19 Jan 2011 13:09:03 +0530 sujay kumar
>
Dear Friends,
i need correct interperation of the Clause of mentioned below.
thanks and regards
QW-407.2
A change in the postweld heat treatment(see QW-407.1) temperature and time range
The procedure qualification test shall be subjected to
PWHT essentially equivalent to that encountered in the
fabrication of production welds, including at least 80% of
the aggregate times at temperature(s). The PWHT total
time(s) at temperature(s) may be applied in one heating
cycle
-->To post to this group, send email to materials-welding@googlegroups.com
>To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
>For more options, visit this group's bolg at http://materials-welding.blogspot.com/
>The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
>
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
Comments