Skip to main content

Re: [MW:29647] Double Normalizing

which hardness was reduced? That of SA387 or that of the cladding?
What was the normalization temp? 900 deg?
Was the cooling after the normalization done at still air or it was done under the insulation? if you heated at 900degC and then cooled slowly under insulation, then you have recrystallized and increased the grain size, so metallurgical properties have been deteriorated 

The cladding risk sensitization if the ss is not stabilized with Ti. You have to check the cladding to check if chromium carbides have precipitate to the grain boundaries

Στις Δευ, 27 Μαΐ 2019 στις 7:01 μ.μ., ο/η Jayesh Parekh <jayeshparekh34@gmail.com> έγραψε:
Recently we faced one issue. Shell side heat exchanger is by mistake subjected to Normalizing in place of PWHT. Material is SA387 Gr.11 Cl2 with 3 mm SS304L Cladding.THickness22mm+3mm cladding.  So due to this hardness is reduced and it is in range of 140 BHN and overall length is increased. For this issue what will be best solution.
Equipment will subject to tempering at 720 deg C for 1 Hr. and then PWHT at 690 deg C for 1 Hour. Due to this heat treatment is there any problem come into materila? Is material property is above minimum required value? What will be effect on SS304L cladding after this much heat treatment? In this condition ,Will equipment suitable for application ? or any other option ? 
Please need expert advice on this issue.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/8daca936-8b7c-4fd6-a1ed-503a8e370f12%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.


--
Dr. Georgios Dilintas,
Dipl. Ing. In Aeronautic and Space Engineering
Ph.D in Mechanics of Solids - Computational Mechanics
A.I.S, A.N.I, IRCA Lead Auditor
Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAPOi40CbBNrOLmT5y2VDdyidZS1kQUPuavtR5Vm8wUZcCYy8NQ%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...