Skip to main content

Re: [MW:29628] Pipe sipport weld joint

Hi,

To contemplate on your scenario, after the butt weld of pipe to elbow, your construction team proceeded welding the shoe on elbow ? So as per your statement it is not just kissing with haz but clashing, which means your construction did intentionally, now you're here for correction.

Yes correction can be done as per your above proposal if your company has any standard stating with the clause or if you have a procedure or write and take approval.

One of world's top company standards clause waives your requirement with what you have proposed.

Check SAES-W-011, search for encroachment.

Thanks 

Muneeb

On Wed, May 22, 2019, 4:10 PM Chiranjeevi A <chiranjeevipuvvula@gmail.com wrote:
Dear George,

We are using ASME B31. 3

On Tue 21 May, 2019, 3:04 PM George Dilintas, <dilintas@gmail.com> wrote:
what is the applicable Code/ Standard (B31.1?, B31.3? other?)

Στις Παρ, 17 Μαΐ 2019 στις 12:18 μ.μ., ο/η Anil <chiranjeevipuvvula@gmail.com> έγραψε:
Dear All,

   In site we have one case that pipe shoe support weld clash with elbow weld, i.e.gap between weld toes is zero.

   Can we proceed with the joints at least 100mm of each welds will be tested with 100% X-ray, 100% VT and 100% MT

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/8bd4bdfa-027b-44c6-96d8-b5bcee41de95%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.


--
Dr. Georgios Dilintas,
Dipl. Ing. In Aeronautic and Space Engineering
Ph.D in Mechanics of Solids - Computational Mechanics
A.I.S, A.N.I, IRCA Lead Auditor
Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAPOi40CYjz8qi%2Bmme2jva18Lh-5uF-gMm%3DUM%3DMuC%3DZdrhvOS-Q%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAN4%2Bm0yELuasmUicGpyssfy7Oa9UbCk3BwbwqLXhfoEZ4GFZqg%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CANtRWKu%2BLxVu7aVNUFfQBmcbqnHZtQ-AH7z4V-XSRFmLGMKPhg%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Re: [MW:14950] RE: 14919] Stress relieving Rejected for 5 min less soaking time.

Dear All, I have been a CONSULTANT FOR such problem & my personal opinion is expressed as follow. I fully agree with views expressed so far. But bag to differ that " Code is a law, with engineering judgments. Hence the inspector has the rights to declare that the original HT was inadequate." Inspectors & total industry must resist the "REJECTION" . We as intellectual & having seniority must become practical. How the code will revise???. ANS.: One is experiments (Pure research) & second is such chances that gives opportunity to experiment !!! _______________________________________________________________________________________________ My understanding is that it is P1 material. In that case every pass normalizes the immediate bottom pass. Hence code requirement for P1 FOR MANDATORY SR is 32 mm & above thickness. SOLUTION:  In any case 0. After SR=PWHT no PTC testing is required as per code--Unless for low temp. vessels. That means code ...