Re: [MW:27051] Required electrode for A335 P11 # S316 material

its design temperature is 500 degree centigrade and working pressure is 68 Bar and the joint is pipe to threadolet and pipe thickness is 14 mm..so plz suggest

On Thu, Nov 23, 2017 at 3:23 PM, 'james gerald' via Materials & Welding <materials-welding@googlegroups.com> wrote:
It depends on the Design Temperature and any PWHT   if Applicable.

Normally for Design temperatures above 315degC or when PWHT is Applicable

1. Choice one is to use ENiCrMo3(Alloy 625 based) butter the P11 side for around 6-8mm and perform the PWHT and weld the buttered end with the 316 using E309MoL/E309L when design temperature is less than 315degC else weld with ENiCrMo3.

Thanks & Regards

J.Gerald Jayakumar

0091-9344954677



On Thursday, November 23, 2017, 1:01:09 PM GMT+4, Chandra Bhanu Mohapatra <bapunchandra@gmail.com> wrote:


Dear Expert 
                       Can somebody help me out to decide the electrode for the pipe welding (Material A335 P11 # S316 ) and Design Code is B31.1

--
tHanks & rEgards
Chandra Bhanu Mohapatra

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.



--
tHanks & rEgards
Chandra Bhanu Mohapatra
8763071417

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...