The nominal / governing thickness is more than 38mm i.e 40mm FPW.
As per UCS 56, PWHT will be required for the 40mm thick lifting lug weld joint.
You should have welded the lifting lug earlier and sent the equipment for PWHT !!
PREM S NAUTIYAL
CELL : 9769316004
From: Muhammed Ibrahim PK <ibratech@gmail.com>
Sent: Wed, 15 Nov 2017 21:28:10
To: materials-welding@googlegroups.com
Subject: [MW:26985] PWHT of lifting lug
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
As per UCS 56, PWHT will be required for the 40mm thick lifting lug weld joint.
You should have welded the lifting lug earlier and sent the equipment for PWHT !!
PREM S NAUTIYAL
CELL : 9769316004
From: Muhammed Ibrahim PK <ibratech@gmail.com>
Sent: Wed, 15 Nov 2017 21:28:10
To: materials-welding@googlegroups.com
Subject: [MW:26985] PWHT of lifting lug
Gents,
I need to clarify one issue with PWHT of a lifting lug.
An ASME Sec VIII Div I vessel require PWHT. lifting lug pad welded with vessel and PWHT done. After PWHT a lifting lug will weld with the pad. The lifting lug having thickness of 40mm and having full penetration groove weld with pad. Is this lifting lug to pad welding required PWHT ?. Please find attached drawing detail for reference.
Your valuable advice will be appreciated.
Thanks & Regards
Muhammed Ibrahim PK
Muhammed Ibrahim PK
| Virus-free. www.avast.com |
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.
Comments