Thursday, December 25, 2014

Re: [MW:22640] FCAW Consumable for Ferritic SS

Dear Mr.Raj,
 
The weldability of X10CrAlSi7 was limited.
 
You can use ER309 filler for the stated combinations.
Preheat (min 200°C) & Interpass (max. 300°C) should be maintained.
Cutting of these materials by thermal process is critical for obtaing good results on mechanical properties.
Low heat input should be used while welding.
 
 

 
On Thu, Nov 6, 2014 at 3:02 PM, Raj Gupta <raj.aryans03@gmail.com> wrote:
Dear Experts,
Plz suggest me a FCAW/GMAW consumable for Ferritic Stainless Steel Grade X10CrAlSi7, Number 1.4713, Standard: EN 10095 to same and a joint with Mild Steel. And What precautions should be taken for welding of Ferritic Stainless Steel. if you have any literature related to weldability of same steel plz provide, it will be very helpful.

Thanks&Regards
Raj   

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.



--
 
 
With Regards
 
 
Srinivasu V
Welding Engineer

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

No comments:

[MW:35692]

Dear all    Can I do MPI above painting surface for cs  tank  Regards, Sriram Srinivasan -- https://materials-welding.blog...