Dear Sir,

I have found some data for Filler Wire from ASME Sec. II Part-C.

The general compositin for you base material is 9Ni (I guess).

Filler Wire details extracted from Sec.II Part-C(SFA-5.14/SFA-5.14M) are as follows:- 

ERNiMo-9. The nominal composition
(wt.-%) of filler metal of this classification is 70 Ni, 20 Mo, 3 W, and 1 Fe. Filler metal of this classification is used
for welding 9% nickel steel (ASTM A 333, A 334, A 353,and A 553 having UNS number K81340) to itself using the GTAW and SAW processes.

You may refer ASME Sec. II Part C for Filler wire specifications.


I am a Novice to all this, so please correct me if I am wrong. Also I am attaching a presentation which I found while browsing through internet. Hope that is useful for you.




On Mon, Oct 28, 2013 at 12:09 AM, Anban <gane2478@hotmail.sg> wrote:
Dear Experts

Pls share your expertise in qualifying PQR
 
ASTM A333 Grade 8 ( UNS K81340 ),

CVN at -195 deg celcius.

P.No- 11A/ Group No - 1.

Min Dia 2" / Max Dia 8".

Min Thk-11.0mm / Max Thk - 32.0mm.




 2" and below - 100% GTAW.


Above 2 " - Intend to Weld Process - GTAW + SMAW , GTAW + FCAW.

Must comply to NACE MR0175.

Advise suitable welding consumable from  ESAB / Lincoln/Sanvik..etc

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.



--
Thanks & Regards,

A Bharat Kumar
+91 9989717650

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...