Dear Pokala Ramu,
 
I have been in the powerplant piping industry where the PWHT will be done on the A335 P91 welds together with the gamma plugs after RT acceptance. This practise is accepted as grain refinement will occur in a homogeneous way and we dont have to subject the same material to PWHT time again and again. If you are worried about deformation, then that is entirely different story.

On Fri, Oct 25, 2013 at 4:34 PM, pokala ramu <pokala.rams@gmail.com> wrote:
Dear All,

We are going to carry out weld repairs on our Amine regenerator column during shutdown. Repair will be carried out by weld build up due to internal corrosion. At the same time there is a modification in the column we are adding two 12"Dia nozzles. at 1meter higher elevation from the weld repair location. Due to service requirement PWHT is mandatory. In order to reduce shutdown window there is a proposal to carry out carry out PWHT on newly added 2 nozzles and the weld repair location at the same time. Is it allowed to carry out the PWHT at the same time?

At Nozzles PWHT will be carried out by Bulls-eye technique and at the weld repair location PWHT will be carried out by circumferential band heating of the complete column.

 Is there going to be any issue with the deformation etc. Kindly share your experience.
the details of the column are as follows:

1. Material: A516 Gr.55
2. Diameter: 4meter
3. Height: 20 meter
4. Thickness: 11mm
5. location of nozzle addition: 4 meter from top
6. location of the weld repair: 5meter from top

Appreciate your advises.

with best regards
Ram Pokala


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.



--
This message originated from the Internet. Its originator may or may not be who they claim to be and the information contained in the message and any attachments may or may not be accurate.

This email transmission is intended solely for the named recipient(s). It may contain confidential and/or privileged information.If you are not the intended recipient, note that disclosing, copying or distributing it may be unlawful. Please notify the sender immediately if you have received it by mistake, and delete it from your system.
Internet communications cannot be guaranteed to be timely, secure, error or virus-free. The sender does not accept liability for any errors or omissions.

"SAVE PAPER - THINK BEFORE YOU PRINT!"

Regards,

~ DEVARAJAN RAMASAMY~

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...