Dear Satish,

 

This is an area of the weld where there is in fact no weld material present. Often referred to as a “hole”.

Rejectable to any code.

 

Kind regards

 

Nick

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Sathish Kumar
Sent: 19 November 2012 11:41 AM
To: materials-welding@googlegroups.com
Subject: [MW:15959] What kind of weld defect? pl advice..

 

Dear experts,

pl find attach.

it is a structure welding. fillet weld.

What kind of defect is this? whether this is acceptable or reject as per spec/code. pl specify exact reference.

thanks in advance.

 

sathish

saudi

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
 
 

No comments:

[MW:34920] Tubesheet Hole step

Hello Team, I have one question any tolerance given for tubesheet Hole step. Please do needful. Regards, AP  -- https://materials-...