RE: [MW:14973] Need WPS clarification with ASME and EN

For EN   -  Variable Essential:

 

Process 12

- Each variant of process 12 (121 to 125) shall be qualified independently.

- The qualification given for the flux is restricted to the make and designation used in the welding  procedure test.

 

Processes 131, 135, 136 and 137

- The qualification given to the shielding gas is restricted to the symbol of the gas according to EN 439.  However, the content of CO2 shall not exceed 10 % of that used to

   qualify   the procedure test. Shielding gases not   covered by EN 439 are restricted to the nominal composition used in the test.

- The qualification given is restricted to the wire system used in the welding procedure test (e.g. singlewire or multiple-wire system).

- For solid and metal cored wires, the qualification using short circuiting transfer (dip) qualifies only short circuiting transfer (dip). Qualification using spray or globular transfer

  qualifies both spray and globular transfer.

 

Process 141

- The qualification given to the shielding gas and backing gas is restricted to the symbol of the gas according to EN 439. Shielding gases not covered by EN 439 are 

  restricted  to   the  nominal composition used in the test.

- A weld procedure test made without a backing gas qualifies a welding procedure with backing gas.

- Welding with filler material does not qualify for welding without filler material or visa versa.

 

Process 15

- Qualification of the welding procedure is restricted to the plasma gas composition used in the welding procedure test.

- The qualification given to the shielding gas and backing gas is restricted to the symbol of the gas according to EN 439. Shielding gases not covered by EN 439 are

   restricted  to   the nominal composition qualified.

- Welding with filler material does not qualify for welding without filler material or visa versa.

 

Process 311

- Welding with filler material does not qualify for welding without filler material or visa versa.
 

 
FOR ASME (SMAW)   - Variable Essential 

.

- Essential Variable                      -  QW403.8 = T Qualified,   QW403.9 =  t Pass > 12 in. (13 mm),  ,QW403.11 =  P-No. qualified

- Supplimentry Essesntial Vriable  -  QW403.5 = Group Number,   ,QW403.6 = T Limits impact


 

- Essential Variable                        -  QW404.4 = F-Number,  QW404.5 = A-Number,   QW404.30 = t
- Supplimentry Essesntial Variable  -  QW404.7  =  Diameter > 14 in. (6 mm),  ,QW404.12  =  Classification
 
- Supplimentry Essesntial Variable  -  QW405.2  = Position
 
- Essential Variable                        - QW406.1  =  Decrease > 100°F (55°C)
 

-
Essential Variable                       - QW407.1   =  PWHT,   QW407.4   = T Limits
- Supplimentry Essesntial Variable  -  QW407.2  = PWHT (T & T range)
 

- Supplimentry Essesntial Variable  -  QW409.1  =  Heat input,  QW409.4 =  Current or polarity
 
- Supplimentry Essesntial Variable  -  QW410.9  = Multiple to single pass/side


 


Thank & Best Regards,

 

MVeera SAMY,

Coimbatore

 

 


 

To: materials-welding@googlegroups.com
Subject: Re: [MW:14960] Need WPS clarification with ASME and EN
From: Vinayak_Kale@Lntenc.com
Date: Thu, 26 Jul 2012 08:36:28 +0530


Can , provided , all essential parameters & properties shall match


Regards


Vinayak Kale
OGSP - QA & I , HC - Upstream
EPC Block , 2nd Floor , Gate No.1
Saki Vihar Rd. Powai Campus
Mumbai - 400072
Ph : + 91 022 6705 3969
(M) - 9987875309
www.larsen toubro.com



[MW:14959] Need WPS clarification with ASME and EN

Naresh Kumar   to: materials-welding@googlegroups.com
07/26/2012 08:34 AM

Sent by: materials-welding@googlegroups.com



From: Naresh Kumar <snareshkumar30@yahoo.com>
To: "materials-welding@googlegroups.com" <materials-welding@googlegroups.com>
Sent by: materials-welding@googlegroups.com
Please respond to materials-welding@googlegroups.com




Dear experts,

I have a doubt about WPS. Our company has WPS with ASTM material by ASME standard.
Whether this WPS can be used for the equivalent BS material or not.
 
 
Thanks & Regards,
Kumar S --
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.


Disclaimer :This email and any files transmitted with it are intended solely for the use of the addressee(s) only and may contain confidential and/or privileged information. If you are not the addressee, then this message is not intended for you and be advised that you have received this email in error and that any use , dissemination , forwarding, printing or copying of this email is strictly prohibited. In such case please notify the sender and delete this email and any attachments with it from your system immediately.Receipt of this email by you shall not give rise to any liability on the part of Larsen & Toubro Limited


--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

Re: [MW:35686] HDPE WPS

Refer ASME SEC IX  There is separate chapter for Plastic welding . Based on that you have to prepare  Sent from my iPhone On 21 Jun 2025, at...