Skip to main content

Re: [MW:10495] RE: 10463] Backing

We are essentially doing GMAw welding on thick plates with single grrove with 2 m root face. . One way of checking penetration is to see whether an uniform  weld metal deposit has appeared on the bootom side. If it has then it is grinded and removed other wise gougins is done and welded again.
I therefore agree that it is not backing.  
Backing is done generally where appraoch from the other side is not available and whre full penetration is the requirement.
Arijoy Roy
R&D Telcon
Jamshedpur

--- On Wed, 23/3/11, Karthik <karthik6684@yahoo.com> wrote:

From: Karthik <karthik6684@yahoo.com>
Subject: Re: [MW:10480] RE: 10463] Backing
To: materials-welding@googlegroups.com
Date: Wednesday, 23 March, 2011, 9:32 PM

I think,this is not a backing,because this is to make sure for the welder confirmation. it is happen in normal practice that after welding of single v groove of plate and to be confirmed by visual to confirm the full penetration..and if the penetration is good...many(All) times the welder need to confirm by themself by grind to some depth after confirm by visual (1 or 2mm max..) to make it look good appearnce as well as to avoid any discrepancies in RT.(even it can accept in Rt without grinding)
 
As far as my experience and Customer,AI witness.. it was accepted as without backing...

Thanks & Regards,

(Karthik)

Karthikeyan.S
QA/QC Manager
Getabec Energy Co.,Ltd.
379,Moo6,Soi8,Nikhomphatana,
Rayong-21180,
Thailand.
Phone: 0066 38 897035-8 (Off)
Fax: 0066 38 897034
Hand Phone: 0066 892512282


--- On Wed, 3/23/11, John Henning <jhenning@deltak.com> wrote:

From: John Henning <jhenning@deltak.com>
Subject: [MW:10464] RE: 10463] Backing
To: materials-welding@googlegroups.com
Date: Wednesday, March 23, 2011, 9:41 PM

YES – it is welding with backing.

 

See QW-402.4, non-essential variable for both SMAW and GMAW and an essential variable for welder performance qualification for both processes per QW-416.

 

"QW-402.4  The deletion or the backing in single  welded groove welds.  Double welded groove welds are considered welding with backing."

 

John

 

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of Venkateswaran
Sent: Wednesday, March 23, 2011 4:11 AM
To: materials-welding@googlegroups.com
Subject: [MW:10463] Backing

 

 

As per ASME SEC IX ,we qualified PQR(SMAW/GMAW process) with 8mm/10 mm thickness plate full penetration welding( Root Land:1mm to 1.5 mm) as root ,hot and cap welding and then back/root side of plate was grounded(approx 2mm) to sound metal and one pass of cap welding was done in root side.

My question is whether is method is considered as welding with backing or with out backing it is considered as backing. how?

 

 

 

Regards,

 

kvr

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...