Re: [MW:10433] Welder's qualification for diffrent steels and steel alloys.

Dear Mr. Gohil,
 
Kindly read the references also from QW 353 and QW 356 , like for P no chage please refer from QW353 to QW403.18 and QW423
For your case, I believe that for both carbon steel and alloy steel welding consumable is F No.6 for GTAW, hence if your welder qualify in carbon steel with F No.6 material , he will be qualified for P No.4 also, provided, other essential varialbles of QW 356 doesn't change ( i.e . diameter, backing, position etc)
 
But for SMAW , carbon steel F No. and alloy steel F No may be different, hence the welder may be not qualified.
 
You have to consider, all the essential variables of QW 353 and QW 356 and also the correspond references.
 
Hope it will clearify youe doubts.
 
Kind Regards,
 
Sukamal Naskar
On Sat, Mar 19, 2011 at 5:08 PM, Narendra Gohil <ngohil@qafco.com.qa> wrote:
Dear Mr. Naskar,

That means mainly we have to follow QW-353(SMAW) or QW 356(GTAW) for welder qualification.And that clearly mentioning P no as essential variable for the base metals.

So here even if  my welder is qualified with CS.I have to go for separate qualification for low alloy steel as P no. is changing.

Kindly correct me if my understanding is not correct.

Thanks & rgds
Narendra Gohil
Welding Engineer
QAFCO
Ph.+974-44228289(O)





From:        Sukamal Naskar <sukamalbecmet@gmail.com>
To:        materials-welding@googlegroups.com
Cc:        Narendra Gohil <ngohil@qafco.com.qa>
Date:        19/03/2011 11:52
Subject:        Re: [MW:10428] Welder's qualification for diffrent steels and steel alloys.
Sent by:        materials-welding@googlegroups.com




Dear Mr. Gohil,
 
Whenever you will qualify any welder, you have to consider all the essential variables QW353, QW356.
 
The F-No will chage for SMAW , and for GTAW may be the F-No wil be same.
 
If all the essential variables of QW 353 (SMAW) and QW 356 (GTAW) dosen't change , then you can qualify the welders accordingly.
 
Kind Regards,
 
Sukamal Naskar
Senior Welding Engineer
Bohler Welding

On Sat, Mar 19, 2011 at 11:36 AM, Narendra Gohil <ngohil@qafco.com.qa> wrote:
Dear Experts,

As per ASME sec.IX- QW423.1 mentioning Base metals for  welder qualification and also mentioning qualified production base metals against that.


Like; P-or S-No.1through P -or S- No.11,P- or S-No. 34,and P- or S-No.41 through P- S-No.49 and against that  same grouping and range of P- or S-No. mentioned for qualified production base metals.


That means if a welder qualified with as for example in CS(P no-1) welding(GTAW or SMAW any one ) with preheating and PWHT welding parameters,he can qualified with Low alloy steel like (P.No.4 or other in low alloy steel).


I have been questioned by our Inspection experts and I don't have answer other than mentioned in QW401.2"essential variable"(Performance).


Thanks & Rgds.

 
Narendra Gohil
Welding Engineer
QAFCO
Ph.
+974-44228289(O)

--
To post to this group, send email to
materials-welding@googlegroups.com
To unsubscribe from this group, send email to
materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.




--
Sukamal

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at
http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.




--
Sukamal

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...