Wednesday, December 15, 2010

Re: [MW:8734] Welding electrode to weld AISI 4140 with AISI 4130

Hi
 
Use ER80SG (Root )/E10018-D2 (Filling& Capping) , with a minimum preheat of 150 deg cel. and
 
PWHT @650 deg. cel and soaking time depending on the hardness requirements  if any.
 
Thanks & Regards,
 
K. Babu
----- Original Message -----
From: Aly
Sent: Wednesday, December 15, 2010 2:48 AM
Subject: [MW:8733] Welding electrode to weld AISI 4140 with AISI 4130

Dear All,
Thank you for your time to read my question.
 
I have to weld grade AISI 4130 with AISI 4140. Weld joint configuration is a groove weld 6inch dia.
 
Which electrode is suitable for welding these base metals together.
 
UTS of these parent metals is around 95 to110 ksi.
 
Thanks
 
Mhaskar Aly
FREE Christmas Animations for your email – by IncrediMail! Click Here!

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

No comments:

[MW:34920] Tubesheet Hole step

Hello Team, I have one question any tolerance given for tubesheet Hole step. Please do needful. Regards, AP  -- https://materials-...