[MW:9006] Re: Groove weld qualification for fillet weld

Dear Manpreet,

For Welder Qualification as per Section IX there is no variable for
Impact . As far as base metal is concerend the only variable is 403.16
& 403.18 in case of SMAW.

As per below extract from ASME Section IX:

QW-303.1 Groove Welds — General. Welders and welding operators who
pass the required tests for groove
welds in the test positions of table QW-461.9 shall be qualified for
the positions of groove welds and fillet welds
shown in table QW-461.9. In addition, welders and welding operators
who pass the required tests for groove welds
shall also be qualified to make fillet welds in all thicknesses and
pipe diameters of any size within the limits of the
welding variables of QW-350 or QW-360, as applicable

Best Regards,

JASPAL SINGH CWI-AWS, CSWIP-3.1
ISGEC-PED, Yamunanagar, Haryana (India) PH: +911732307251 ; Mob.
+918930111441(CUG), +919996624244
www.isgec.com

On Dec 30, 7:54 am, "manpreet " <manpreetsi...@rediffmail.com> wrote:
> Dear All,According to QW-451.4, Groove weld qualifies for all thickness ranges of fillet welds,In production a a fillet joint with 25mm &amp; 13mm, impact test required,Is the code saying that QW-403.6 &amp; QW-451.1 will not be applicable here? Please give me your views.....RegardsManpreet Singh

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...