Re: [MW:9027] Re: Stress Corrosion Cracking Test


Dear Mr. Herman

Thanks for quick reply.

It is not mistake in specification. Specification categorically demands 40% CaCl2 solution (Ph -6.5, Testing time - 500 Hrs., 100 Deg Boiling, Acceptance criteria - Stress to cause rupture shall exceed 0.85 times UTS, as per ASTM G 46)

Further, specification calls for  MgCl2 solution for Duplex grade as per G 36.

Since, aberrant solution is being asked for testing as per ASTM G 36, precisely the question was put in this forum.

Request all team members to share views of chloride stress corrosion test of super Duplex ( S 32750)

With Best Regards,

Jignesh R Rana
Manager - QA & QC

Linde Engineering India Pvt. Ltd.
38, Nutan Bharat Society, Alkapuri, Vadodara 390007, India
Tel.: +91 265 3056789, Fax: +91 265 2335213 , Mobil:  +91 90999 86019
jignesh.rana@linde-le.com, www.linde-india.com

This e-mail is confidential. If you are not the intended recipient, please notify us immediately. You should not disclose its contents to any other person nor use it for any purposes.





hpi001 <pieper-qsi@kpnmail.nl>
Sent by: materials-welding@googlegroups.com

30/12/10 16:53

Please respond to
materials-welding@googlegroups.com

To
"Materials & Welding" <materials-welding@googlegroups.com>
cc
Subject
[MW:9019] Re: Stress Corrosion Cracking Test





Why does anyone asking for ASTM G36 with an aberrant test solution?
Probably there will be no big difference between both solutions
because Chloride is the important part in this test but by choosing
for CaCl you won't have any reference or acceptance criteria or is
this also specified in the project specification? Can it be a mistake
in the specification as well?

Best Regards,

Herman Pieper

On 30 dec, 11:44, jignesh.r...@Linde-LE.com wrote:
> Dear Members,
>
> One of our project specification calls for Chloride Stress Corrosion
> Cracking as the ASTM G 36 with CaCl2 (40%) solution for super Duplex
> Stainless steel ( S 32750)
>
> ASTM G- 36 is based on MgCl2 solution.
>
> Does any one having experience with SCCT with CaCl2 solution ?
>
> With Best Regards,
>
> Jignesh R Rana
> Manager - QA & QC
>
> Linde Engineering India Pvt. Ltd.
> 38, Nutan Bharat Society, Alkapuri, Vadodara 390007, India
> Tel.: +91 265 3056789, Fax: +91 265 2335213 , Mobil:  +91 90999 86019
> jignesh.r...@linde-le.com,www.linde-india.com
>
> This e-mail is confidential. If you are not the intended recipient, please
> notify us immediately. You should not disclose its contents to any other
> person nor use it for any purposes.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

--
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Comments

Popular posts from this blog

Materails FAQs

Q: What are equivalents for standard Q 235 B (and Q 235 A) for U-channels? (asked by: boris.vielhaber@vait.com) A: DIN Nr. = 2393 T.2, 2394 T.2, EN 10025 W. Nr. DIN 17007 = 1.0038 Design DIN 17006 = RSt 37-2, S235JRG2 (Fe 360 B) Q: What is St DIN 2391 BK material? (asked by: dmcandrews@automaticstamp.com) A: Precision steel tubes, cold-finished/hard. Q: What is C.D.W. Boiler Tube? (asked by: montydude123@yahoo.com) A: Cold Drawn Welded Boiler Tube. Q: WHAT IS W.Nr. 1.4301? PLS TELL US IN EASY LANGUAGUE (asked...

[MW:36169] Cold Bending Qualification

Dear Experts,  Can anyone share the inspection requirements or a qualification procedure for cold bending? Our client spec states only the requirements for induction bending and would like to know your opinion on the cold bend inspection requirements. The code of construction is B31.3, Max. 5D bends, A106 SS 316L.  Thanks in Advance. -- https://materials-welding.blogspot.com/ https://www.linkedin.com/groups/122787 --- You received this message because you are subscribed to the Google Groups "Materials & Welding" group. To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com . To view this discussion visit https://groups.google.com/d/msgid/materials-welding/1be61cc3-e9c9-4a5f-834d-e8485e248432n%40googlegroups.com .

Heat tint (temper) colours on stainless steel surfaces heated in air // Heat tint

Introduction The colour formed when stainless steel is heated, either in a furnace application or in the heat affected zone of welds, is dependent on several factors that are related to the oxidation resistance of the steel. The heat tint or temper colour formed is caused by the progressive thickening of the surface oxide layer and so, as temperature is increased, the colours change.   Oxidation resistance of stainless steels However, there are several factors that affect the degree of colour change and so there is no a single table of colour and temperature that represents all cases. The colours formed can only be used as an indication of the temperature to which the steel has been heated. Factors affecting the heat tint colours formed Steel composition The chromium content is the most important single factor affecting oxidation resistance. The higher the chromium, the more heat resistant the steel and so the development of the heat tint colou...