difficult to weld oxygen bearing copper
Some times CuSi type filers are an added advantage due to its fluidity,
consult a consumable manufacturer with correct type/grade or UNS# of the
material
Helium (or He+Ar mixture) can be selected as a shielding gas because;
risk of oxide entrapment in the weld pool is greatly reduced and
provides deeper penetration
Preheating of the base metal is typically required to maintain the base
metal at welding temperatures without preheating, the high thermal
conductivity of copper results in excessive loss of heat away from the
weld zone.
-----Original Message-----
From: materials-welding@googlegroups.com
[mailto:materials-welding@googlegroups.com] On Behalf Of gajjalla surya
prakash
Sent: Wednesday, September 30, 2009 11:47 AM
To: materials-welding@googlegroups.com
Subject: [MW:3373] filler wire for copper
dear all ,
can any one suggest me the filler wire for GTAW process for weld 12mm
thk Pure copper to copper plate(99.3%)
--
With regards,
Surya Prakash Gajjalla
Filtered by Hosted Filtering
--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---
Comments