Tuesday, September 15, 2009

[MW:3204] Re: Filler for TP304H toA335 P11

Dear Mr.Shanmugam,
 
The response of Mr Amarjit Singh is correct. I would like to add a bit of additional info on to this.
 
API-582,Recommended Practice-Welding Guidelines for Chemical,Oil and Gas Industries , clause 6.2 (On Dissimilar metals welding) privides a table and further recommendations on dimmilar metals welding in petrochemical environment. You may download the draft for Ballotting (free copy) from API website or alternatively buy it through API.
 
Thanks
 
Pradip Goswami
Welding/Metallurgical Engineer/Specialist
Ontario Power Generation Inc.
Ontario,Caanada
 
 

 

Date: Sun, 13 Sep 2009 21:00:34 +0530
Subject: [MW:3195] Re: Filler for TP304H toA335 P11
From: amritas2001@gmail.com
To: materials-welding@googlegroups.com

Dear Mr.Shanmugam

Since the operating temperature is below 325 deg C , you can use E309L/ E309MoL consumable. If the operating temperature is more than 315deg C , then have to use inconel electrodes e.g. ENiCrMo-3.
 
Regards,
Amarjit Singh

On Mon, Sep 7, 2009 at 11:59 PM, Siva Shanmugam <siva196510@gmail.com> wrote:

Dear all,

I would like to know your suggestions about the filler materials for
welding of TP304H to A335 P11 for natural gas feed stock in reformer
with the working temperature around 250 deg.celcius.

Welcome for all of your valuable recommendations and suggestions.

Best regards,

R.Sivashanmugam


--
Amarjit Singh

--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

No comments: