[MW:3181] Re: Weld over lay on the inner surface of an elbow

Yes , you can have the hardfacing on the inner surface with stainless steel material. But the austenitica SS are not good for erosion. For better erosion resistance you need to choose martensitic SS overlay or matensitic steel alloys
 
amarjit singh

On Tue, Sep 8, 2009 at 9:33 AM, Chandulal Vithlani <chandulal.vithlani@borouge.com> wrote:

We have a problem of erosion by steam + water jet.

 

Material of the elbow is A234-WPBW Thickness: 0.75" Diameter: 28" Long Radius

 

We would like to have hard facing on the inner surface without the need for PWHT.

 

 

Can any one suggest suitable WPS for the same?

 

Regards

 

Chandulal S Vithlani

 

 

 

 

**********************************************************************

Borouge is a leading provider of value creating, innovative plastics solutions for customers in the Middle East, Asia-Pacific and Africa. Borouge employs unique Borstar® technology to produce differentiated products for high-value infrastructure applications, including water, gas and industrial pipe systems, power and communication cables, advanced packaging and automotive components. Borouge's state-of-the-art petrochemical complex is located at Ruwais, Abu Dhabi in the United Arab Emirates.

===================================================================================
CONFIDENTIALITY NOTICE

This email and any files transmitted with it are confidential and intended solely for the use of the individual or entity to whom they are addressed. If you have received this email in error please delete the email and any attachment(s) and notify the sender.

This footnote also confirms that this email message has been scanned for the presence of computer viruses.
=============================================================================================================

 






--
Amarjit Singh

--~--~---------~--~----~------------~-------~--~----~
To post to this group, send email to materials-welding@googlegroups.com
To unsubscribe from this group, send email to materials-welding-unsubscribe@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
-~----------~----~----~----~------~----~------~--~---

No comments:

[MW:34919] Welder qualification certificate

Dear All     anyone can share a format for welder certificate and card format        Thanks & Best Regards Saleem manhappulath Mob:+9665...